Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

A Comprehensive Understanding of 'TiO2 Pigment Durability'

July 1, 2005
Coatings manufacturers consume nearly three million tonnes of TiO2 pigments globally every year - a clear indication of the importance of this opacifying pigment to this industry. This reflects the unsurpassed ability of TiO2 to uniformly scatter white light without absorption (which would lead to color). Virtually all coatings, except those that are clear or black, take advantage of the opacity of TiO2 as the primary or, in many cases, the only provider of hiding power. TiO2 pigments have a rich history in the coatings industry - a history that goes back over 70 years - and are certain to maintain dominance for the foreseeable future since there are no known not-in-kind replacements that approach the opacity of TiO2.

While the benefits that TiO2 pigments bring to coatings are significant, there are some situations where TiO2 can be harmful to important properties of the final paint film. Perhaps the most familiar example of this to many paint formulators - particularly those who work in the industrial and/or OEM finishes - is the detrimental effect of TiO2 on paint durability. This effect, commonly referred to as "TiO2 durability" (which is actually a misnomer, since the TiO2 itself is completely durable - and hence the quotation marks in the title of this paper), is well recognized in the coatings industry. What is less well understood is that TiO2 affects paint durability in a number of ways, both good and bad. In this paper we review the many ways that TiO2 can affect paint durability, and how the interplay ultimately determines the longevity of a paint film.

Photocatalytic Degradation

Titanium dioxide is an excellent absorber of ultraviolet light, and a single, quarter-micron particle of TiO2 will absorb in excess of 99% of all solar UV radiation that strikes it. The UV light energy is temporarily transformed into electronic energy in the form of an electronically excited TiO2 particle, and then the vast majority of this energy gets quickly converted into heat energy. The heat energy then dissipates from the paint film.

However, for every million light absorption events, anywhere from 1 to 10 will proceed through a different pathway. The energy contained in the excited TiO2 particle is transported to the pigment surface, where it can encounter absorbed water and oxygen. The resulting reaction transforms the energy yet again, this time into reactive chemical energy in the form of hydroxyl and superoxide radicals (Figure 1). These radicals are free to migrate from the pigment surface and react with polymeric resin molecules, ultimately leading to the destruction of the organic component of the paint film.

Photocatalytic degradation of organic binder can be prevented by taking advantage of the fact that it proceeds through a series of chemical reactions - one followed by the next - and that by preventing only one of these reactions, the entire sequence will be stopped. Coatings manufacturers can use additives that prevent the adsorption of UV light by TiO2 (e. g., UV light absorbers) or that prevent the reaction of the photogenerated hydroxyl and superoxide radicals with the binder (e.g., hindered amine light stabilizers - HALS).

While effective, these remedies add cost to the coatings, and the preferred route to reduced photocatalytic activity is for the pigment manufacturers to alter the pigment before it gets into the coating. They do this by completely covering the pigment surface with a layer of inert oxide (silica or alumina), which physically separates the absorbed water and oxygen from the TiO2 crystal (Figure 2).

The Beneficial Effects of TiO2 on Durability

Most formulators are familiar with the detrimental photocatalytic effect of TiO2 on resin weatherability. However, TiO2 can have a very beneficial effect as well. This is because there is another set of degradation reactions that involve UV light, and TiO2 can affect the rates of these reactions.

This set of reactions, termed direct degradation, involves the direct absorption of UV light by the resin polymer. UV light photons are so energetic that this absorption event often causes weak chemical bonds within the resin to break (e. g., C-H bonds). The yield per photon for these reactions is typically many orders of magnitude greater than the yield per photon for photocatalytic degradations - that is, a UV light photon directly absorbed by the resin polymer is much more likely to cause damage than one that is absorbed by a TiO2 particle.

TiO2 pigment does not participate directly in this second set of reactions, but it does have a dramatic effect on their rates. This is because, as mentioned above, TiO2 is an excellent UV light absorber. By removing the UV component of sunlight, the TiO2 particles shield the binder molecules beneath them from direct degradation. This effectively limits direct degradation to the topmost layer of binder molecules.

A Balancing Act

TiO2 has both positive and negative influences on paint film durability. A reasonable question to ask is: which is stronger? That is, does adding TiO2 to a paint improve its durability (due to TiO2 protection of the binder), or hurt its durability (due to photocatalytic degradation)? The simple answer is that for all but the most durable binders (i.e., the ones inherently resistant to direct degradation), the positive influence of TiO2 on durability more than outweighs its negative effects.

A dramatic example of this beneficial effect can be found in the plastics industry. The vinyl used in vinyl siding is typically very susceptible to degradation via direct absorption of UV light, and vinyl siding without TiO2 would last for no more than one or two summers. However, the incorporation of only a few percent TiO2 into the vinyl allows for this product to be warranted for 10, 20 and, in some cases, even up to 30 years. While resin molecules used in paints are not nearly this susceptible to direct degradation, it is true that in most cases the TiO2 pigment has a net beneficial effect, especially when a durable or superdurable grade such as Ti-Pure® R-960 or Ti-Select® TS-6200 is used.

Other Considerations

The effect of TiO2 on paint durability is more complicated than just its effect on resin degradation rates. Paint consumers typically interpret durability in terms of the retention of appearance, and not, necessarily, as a resistance to chemical reaction. While the latter usually influences the former, the degree of influence can vary depending on the grade of TiO2. Said another way, a realistic durability goal for the paint manufacturer is to allow the film to "age gracefully," rather than to completely prevent degradation (which is impossible). By age gracefully, we mean that for a given amount of degradation (as measured by, say, weight loss), the degree to which film appearance changes should be minor. This relationship between amount of degradation and degree of appearance change is found to vary from one TiO2 grade to another.

This is shown schematically in Figure 3 for two paints that differ only in the grade of TiO2 used. In a typical durability study we measure gloss loss as a function of exposure time, but in the idealized graph in Figure 3 we instead follow it as a function of weight loss per unit area. At a given weight loss, Paint A suffers less gloss loss than Paint B. Based on this, a consumer would say that Paint A was the more durable, even though both paints have experienced the same amount of degradation.

What causes this variance, and how can a paint formulator take advantage of it? In the case of gloss, the variance is due to the effect of increasing pigment concentration near the film surface as the resin degrades. As mentioned above, most resin degradation, whether photocatalytic or direct, occurs near the film surface. As the resin degrades it erodes from the paint, primarily by being washed out during cleaning or exposure to rain. The TiO2 pigment is inert and remains behind in the film. The net effect is an increase in pigment volume concentration (PVC) in the immediate vicinity of the film surface (Figure 4).

Paint gloss typically decreases with increasing PVC, and this decrease is especially severe as PVC passes above critical (CPVC). Therefore, any property of the TiO2 or of the paint film that affects the point at which CPVC is reached will also affect the relationship between amount of degradation and degree of appearance change. Paint properties that affect the amount of degradation needed before CPVC is breached include initial PVC (paints formulated near CPVC will show faster gloss loss than paints formulated at lower PVC) and the amount of non-TiO2 pigment and/or filler present. The TiO2 pigment property that most affects CPVC is degree of dispersion. In general, a more poorly dispersed TiO2 (or a more difficult to disperse grade) will have a lower CPVC, and thus show more appearance change with time, than a better/easier dispersing grade. Therefore, the coatings manufacturer should choose, all else being equal, a more easily dispersed pigment for durable paint applications.

Good pigment dispersion also minimizes the rate of gloss loss in another way, in what can be thought of as a "tip of the iceberg" effect. Gloss is essentially a measure of film smoothness on the optical scale - roughly 1/2 micron. TiO2 pigment agglomerates exceed this size, and their presence near the topmost film surface hurts gloss. In the freshly applied paint, this negative effect is minimized by leveling of the resin above the agglomerates. At most, the agglomerates will cause a small bump or ripple on the actual paint surface. However, once the resin begins to degrade, what was once a small bump can quickly become a large surface defect. Initially only the "tip of the iceberg" was affecting surface optics - now the whole iceberg is exposed! If the pigment is initially well dispersed, though, this effect will be minimal since there are no large objects to expose (Figure 5), even if the overall amount of resin loss is the same. So once again we find that all other things being equal, a more easily dispersed pigment will appear more durable (suffer less change in appearance) than one that does not disperse well.

Choosing the Right Superdurable Pigment

Successful development of a superdurable paint is one of the greatest challenges a paint formulator can face. Nearly every ingredient must be carefully chosen to ensure the highest level of durability and to provide other film properties that may be important for the particular application (e.g., gloss or distinctness of image). This is especially true of the grade of TiO2 chosen. When considering TiO2 grades, it is important to look beyond photocatalytic activity - low photocatalytic activity is essential, but other properties of the pigment also affect paint durability. All else being equal, an easily and completely dispersed pigment will provide the best resistance to change in appearance because it will allow any degradation that does occur to have a minimal impact on paint gloss and distinctness of image. Paint formulators should consult with their pigment manufacturer so that a holistic approach is used and the proper superdurable TiO2 grade is chosen for the specific application under consideration.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Paint and Coating Market Reports
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • TZMI Releases Annual Review of TiO2 Pigment Market

    See More
  • TZMI Releases Annual Review of TiO2 Pigment Market

    See More
  • Argex Names Leader of TiO2 Pigment Development Team

    See More

Related Products

See More Products
  • durability.jpg

    Increasing the Durability of Paint and Varnish Coatings in Building Products and Construction 1st Edition

  • Pigment Dispersion (Virtual Course - 11/19/26)

See More Products
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing