Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Zero-Voc, Water-Based Epoxy Topcoat

By Wendy Zhao
March 1, 2010
It is clear that laws governing the use of VOC-containing coatings are becoming increasingly more stringent. For example, the maximum permissible level of VOC for Essential Public Service Coatings in California has been 100 g/L since July 1, 2006. It is reasonable to expect that other states will eventually enact similar legislation. For coatings manufacturers, future success depends upon the availability of products that have low levels of VOC; these products will provide a safer workplace for applicators and result in a cleaner environment.

Since 1982, when the first bisphenol A-based solid epoxy dispersion and modified amine system came to market as an adduct suitable for metal protection, water-based epoxy systems have been used for high-performance industrial primers and topcoats over metal due to their fast dry time, corrosion resistance, good pot life and low odor. Although water-based epoxies have successfully replaced traditional solvent-based epoxy/polyamide coatings in many high-performance industrial applications, the VOC content of these water-based epoxies is typically 200-350 g/L. So now, even though water-based, the usage of these coatings is increasingly limited by VOC regulations.

The technical challenge of developing low- to zero-VOC water-based epoxies is a difficult and complex task that involves attention to the total formulation and all of its compositional materials including resins, pigments and additives. Unfortunately, most water-based epoxies containing very low levels of solvent do not exhibit the same performance as do the heavy-duty solvent-based epoxies and high-VOC water-based epoxies. Major differences are evident in film formation and application properties.

A zero-VOC water-based epoxy topcoat has been formulated without aid of solvent, acid, diluent or plasticizer. It is based on a new innovative bisphenol-A “1”-type solid epoxy resin dispersion cured with modified amine. The new development offers high gloss, fast cure, long pot life and excellent resistance to water, humidity, chemical and corrosion on metal and concrete substrates. The performance properties of the new zero-VOC water-based epoxy topcoat are comparable to solvent-based epoxy/polyamide and high-VOC water-based epoxies.2

Credit: The Sherwin Williams Company
Table 1 Click to enlarge

Experiment and Discussion

Binder System
Water-based epoxies used in conventional protective coating formulations are based on two principal technologies, i.e., liquid epoxy self-emulsifying systems and solid epoxy dispersion systems (Table 1). With epoxy equivalent weight ranging from 175 to 240, liquid epoxy self-emulsifying systems are very rich in epoxide groups. The combination of concentrated epoxides and amine hydrogens in the same emulsion particle provides coatings with high crosslink density and good chemical and abrasion resistance, but very short usable pot life, low flexibility and low impact resistance. These films are often too brittle for use on metal substrates. Since the film formation of liquid epoxy emulsion is dependent upon chemical reaction to increase viscosity, the dry time is very slow, often taking more than six hours to reach a tack-free state.(¹) These liquid epoxy coatings do exhibit good handling, flow and coalescence without the aid of co-solvents, and can often be formulated to very low or zero VOC.

Systems based on solid epoxy dispersion technology offer much faster dry times due to coalescence of the epoxy particles through water and co-solvent evaporation. Solid epoxy resins, with equivalent weights ranging from 500 to 800, provide coatings with lower crosslink density films that are more flexible, adhere better and have better impact resistance than liquid epoxy systems. Pot life is much longer due to the lower concentration of epoxides and amine hydrogens. Solid epoxy dispersion systems are closer in performance, especially on metal substrates, to traditional solvent-based epoxy polyamide systems. The major weakness of the epoxy dispersion type of system is its tendency to form heterogeneous films with epoxy-rich and amine-rich domains due to incomplete coalescence. To aid in processing and to overcome the poor flow and coalescence of the solid epoxy, co-solvents have to be added to the dispersion thereby eliminating any possibility of a zero-VOC formulation.(¹)

A new and innovative solid epoxy dispersion topcoat, cured with a modified water-soluble amine binder system, incorporates the best characteristics of liquid epoxy emulsion and solid epoxy dispersion technologies and can be formulated to zero VOC. It is based on a bisphenol-A “1”-type solid epoxy (EEW 500) using an internal surfactant built into the epoxy resin. When reacted, the internal surfactant becomes epoxy functional and is non-leachable, resulting in cured films with very good water resistance. A unique and patented high-speed dispersion process used for production of the epoxy dispersion yields a very small particle size (0.4 microns) without adding solvents or reactive diluents, providing good film formation, good storage stability properties and low to zero VOC formulation capability. The new zero-VOC water-based epoxy topcoat formulated with this binder system exhibits long pot-life (5.5 h @ 77 ºF/50% R. H.), short dry time (2 h tack free @ 77 ºF/50% R. H.), very good corrosion resistance (4,000 h salt fog) and good chemical resistance.

Credit: The Sherwin Williams Company
Figure 1 Click to enlarge

Pot Life and Film Formation
Unlike solvent-based systems, termination of pot life in many water-based epoxy coatings is not always indicated by a gradual increase in viscosity. Early water-based epoxy systems suffered from overly rapid cure rates and poor gloss and color stability during pot life. The catalyzed paint would exhibit a time related, slow degradation in gloss as in-pot cure advanced during application. This degradation gave variability and patchiness of the coated product, especially in cut-in perimeter areas on large architectural applications.

Credit: The Sherwin Williams Company
Table 10 Click to enlarge

These areas sometimes showed up as patches with non-uniform gloss and color after being filled in by roller application or otherwise touched up at different intervals after mixing. The pot life of water-based epoxy coatings is influenced by a number of factors, such as emulsion particle size, the chemical nature of the epoxy resin and curing agent and the equivalent weight of both the epoxy resin and the curing agent. In general, pre-emulsified, small-particle-size, high-epoxy-equivalent-weight resins give the longest pot life. In some systems, attempts to improve curing agent dispersion and extend pot life by the addition of volatile acid such as acetic acid have been successful. However, unless the amount of acid is carefully controlled, both water and corrosion resistance can suffer. The curing agent is blocked by acids that subsequently evaporate from the applied film to release the amine for reaction with the epoxy. Because the curing agent is blocked, this approach reduces cure rates.

Credit: The Sherwin Williams Company
Table 11 Click to enlarge
Credit: The Sherwin Williams Company
Table 2 Click to enlarge

Pot life was evaluated on the new zero-VOC water-based epoxy topcoat versus a commercialized water-based epoxy topcoat using a solid epoxy dispersion system by measuring viscosity, gloss and color change periodically after initial mixing of the epoxy and curing agent components. End of pot life was deemed the point where the catalyzed coating rose above 120 KU or exhibited a sharp gloss reduction and/or significant color change. Test results, shown in Figure 1 and Table 2, indicate that due to the ultra-fine particle size and the internal surfactant built onto the epoxy resin, the new zero-VOC water-based epoxy topcoat exhibits a long pot life and very good gloss and color stability throughout the pot life. These properties make it an ideal product for large area applications.

Credit: The Sherwin Williams Company
Table 12 Click to enlarge


Thixotropes and Pigmentation

Credit: The Sherwin Williams Company
Table 13 Click to enlarge

Dry film thickness requirements for water-based industrial maintenance topcoat applications are typically in the range of 2 to 5 mils requiring wet film capability of 5 to 12 mils. For the new zero-VOC water-based epoxy formulation, achieving optimum flow and sag control without the benefits of large organic solvent amounts is a difficult task requiring the formulator to rely more on coating additives. Although conventional types of thixotropes used in other water-based coatings, such as bentonite clays, cellulosics (HEC, HMHEC), alkali-swellable polymers (ASE, HASE) and hydrophobically modified urethane associative (HEUR) thickeners can be used, the selection of thixotropes as well as the balance between thixotropy and flow control for the new zero-VOC water-based epoxy system is extremely critical.

Credit: The Sherwin Williams Company
Table 14 Click to enlarge

Thixotropes that introduce any degree of real viscosity are counterproductive. Certain types of surfactants and emulsifiers added to the epoxy and amine resins during the dispersion or emulsion process significantly reduce the thixotropic efficiencies of associative thickeners. Conventional powder thixotropes, such as the bentonite clays, silicas and the high-molecular-weight cellulosics, are often problematic in water-based epoxy formulations, especially when a high-gloss finish is required, so the selection of these materials is limited. The zero-VOC water-based formulation relies on a carefully balanced blend of flow control agents, thixotropes and formula pigmentation to achieve the desired film properties and required sag resistance.

Credit: The Sherwin Williams Company
Table 3 Click to enlarge
Image Caption
Table 9 Click to enlarge

Pigments used in the formulation of the zero-VOC water-based epoxy, including color and hiding pigments, anti-corrosive pigments and extenders used for specific functional purposes, can also cause increased paint viscosity. This makes optimization of formula pigmentation, together with all other formula ingredients, a very complex task. With water-based epoxy formulations, sometimes the epoxy dispersion is pigmented and sometimes the amine curing agent is pigmented. However, in any two-component system, the choice of which component to pigment is normally governed by desired mix ratio. Pigmenting the larger component is always preferred. This makes it much easier for the mixed paint to maintain a full body viscosity and achieve optimal hiding power.

The innovative solid epoxy dispersion used in the new zero-VOC water-based epoxy topcoat has an internal epoxy-functional surfactant built onto the polymer backbone that has proven to have less tendency to reduce the efficiencies of thickeners compared to water-soluble amine or older, solid epoxy dispersion technologies (Table 3). A combination of organic and inorganic thickeners package is used to optimize sag resistance of the paint film. Pigmenting in the epoxy dispersion, the larger component in the 4:1 mix ratio of the new zero-VOC water-based epoxy topcoat, results in full body viscosity and optimized hiding power of the mixed paint. A flow/leveling agent is used along with the high-efficiency thickeners to balance thixotropy and flow control. With all the above successful strategies adopted in the formulation, the new zero-VOC water-based epoxy topcoat achieved the desired film properties with good sag resistance (12 mils wet) and flow properties.

Credit: The Sherwin Williams Company
Table 4 Click to enlarge

Coating Performance

Mechanical Properties

Credit: The Sherwin Williams Company
Table 5 Click to enlarge

The zero-VOC W/B epoxy topcoat described in this paper has excellent mechanical properties as shown in Tables 4, 5 and Figure 2.

Early Moisture Resistance
The new zero-VOC water-based epoxy topcoat has very good early moisture resistance as tested in a mist box.

Credit: The Sherwin Williams Company
Figure 2 Click to enlarge

This test determines the effect of water misting on an applied coating film during various stages of the coating cure cycle. The mist box cabinet is equipped with six fog nozzles utilizing tap water and has a panel rack for supporting test specimens at an angle of 30º from vertical. After the coating is applied at recommended film thickness, samples cured for 2, 4 and 6 h and longer intervals if necessary, are exposed to the mist cabinet for 24 h.

The panels are removed from the mist box and compared to control panels cured at 77 ºF and 50% R.H. Degree of blistering is checked immediately and after recovery using ASTM D 714. Gloss readings are taken according to ASTM D 523 and compared to the control panels. Adhesion checks per ASTM D 3359 are made at 1 and 24 h recovery periods. The zero-VOC water-based epoxy topcoat showed excellent early moisture resistance after only 2 h cure (Table 6).

Credit: The Sherwin Williams Company
Figure 3 Click to enlarge

Under these conditions, the zero-VOC W/B epoxy gloss topcoat showed excellent gloss retention of greater than 70% after 500 h exposure (Table 7 and Figure 3) and color change of less than 5.0 delta-E (Table 8 and Figure 4).

Credit: The Sherwin Williams Company
Table 6 Click to enlarge

This is significantly better performance than seen with the commercial W/B epoxy topcoat.

Corrosion Weathering Resistance
ASTM D 5894 describes a cyclic weathering test that includes wet/dry and light/dark cycles to mimic natural exposures. Test panels are exposed to alternating periods of one week in a QUV chamber and one week in a cyclic fog/dry chamber.

Credit: The Sherwin Williams Company
Figure 4 Click to enlarge
Credit: The Sherwin Williams Company
Table 8 Click to enlarge

The new zero-VOC water-based epoxy topcoat applied over the commercial water-based epoxy primer was rated as 10 with no blistering and no rusting, and scribe performance was rated as 9 with 1/64th inch scribe creep after 10 cycles (Table 9, Figure 5).

Credit: The Sherwin Williams Company
Figure 5 Click to enlarge

This performance is comparable to the commercial water-based epoxy topcoat/primer system and commercial solvent-based epoxy topcoat/primer system (Figure 6).

The zero-VOC water-based epoxy topcoat applied with two coats over sand blasted steel was rated as 10 with no blistering and no rusting after 15 cycles.

Credit: The Sherwin Williams Company
Figure 6 Click to enlarge

The scribe performance was rated as 8 with 1/32th inch scribe creep (Table 10, Figure 7).

Credit: The Sherwin Williams Company
Figure 7 Click to enlarge

In this test, the performance was significantly better than the commercial water-based epoxy topcoat (Figure 8).

Salt Fog Resistance
The salt fog test run is according to ASTM B 117; the test panels are continuously exposed in the cabinet with a wet and dark salt fog environment. The fogging electrolyte solution consists of 5% sodium chloride sprayed at 95 °F (35 °C).

Credit: The Sherwin Williams Company
Figure 8 Click to enlarge

The zero-VOC water-based epoxy topcoat applied over the commercial water-based epoxy primer was rated as 10 with no blistering and no rusting, and scribe performance was rated as 8 with 1/32th inch scribe creep after 2000 h (Table 11, Figure 9).

This performance is comparable to the commercial water-based epoxy topcoat/primer system and commercial solvent-based epoxy topcoat/primer system (Figure 10).

Credit: The Sherwin Williams Company
Figure 9 Click to enlarge

The new zero-VOC water-based epoxy topcoat applied with two coats over sandblasted steel was rated as 10 with no blistering and no rusting after 4000 h.

Credit: The Sherwin Williams Company
Figure 10 Click to enlarge

 In this test, the performance was significantly better than the commercial water-based epoxy topcoat (Figure 12).

Chemical Resistance
The new zero-VOC water-based epoxy topcoat has excellent resistance to a wide variety of industrial and household chemicals. Results of chemical resistance spot tests run in accordance with ASTM D 1308 (Table 13) shows the zero-VOC epoxy topcoat resists acids, bases, industrial solvents such as ketones, alcohols, glycol ethers, and aliphatic and aromatic hydrocarbons and various other chemicals such as bleach, motor oil and brake fluid.

Credit: The Sherwin Williams Company
Figure 11 Click to enlarge
Credit: The Sherwin Williams Company
Figure 12 Click to enlarge

Recommended Systems
The new zero-VOC water-based epoxy topcoat can be applied directly to concrete, metal and primed substrates. The coating is compatible with a wide variety of primers including water-based acrylics, water-based epoxies and solvent-based epoxies. These systems offer comparable exterior durability and corrosion resistance to high-VOC water-based epoxy topcoat/primer systems and solvent-based epoxy topcoat/primer systems. Table 14 shows examples of recommended systems.

Conclusion

A zero-VOC water-based epoxy topcoat has been formulated based on a new innovative solid epoxy resin dispersion cured with modified water-soluble amine without adding solvent, acid, diluent and plasticizer. The new development offers high gloss, fast cure, long pot life and excellent resistance to water, humidity, chemical and corrosion on metal and concrete substrates, making it suitable for many industrial maintenance applications. The performance properties of the new zero-VOC water-based epoxy topcoat are comparable to solvent-based and high-VOC water-based epoxies. The new zero-VOC water-based epoxy offers an excellent alternative to replace conventional epoxy coatings when VOC regulation compliance is critical.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

The Sherwin Williams Company, Chicago, IL

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • pci0421-Aditya-889570808-900.jpg

    Water-Based Epoxy Technologies for Metal Coating Applications

    See More
  • Industry's First Water-Based Epoxy Floor Coating System for Static Control

    See More
  • Water-Based Epoxy Coating

    See More

Related Products

See More Products
  • biopolymer.jpg

    Biopolymer-Based Films and Coatings Trends and Challenges

  • pci january 2020

    PCI January 2020 Issue

See More Products
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing