Paint & Coatings Industry
 HOME
 Subscribe
 E-Newsletter Subscription
 E-Newsletter Archive
 Subscription Customer Service
 Digital Editions
 China Digital Editions
 Finishing Today Digital Editions
 SUPPLIER INFO
 Ad Index
 Buyers Guide
 Online Exhibits
 Virtual Coatings Brochures
 Supplier Price Alerts
 Supplier Request Form
 Videos/PCI TV
 MAGAZINE
 PCI 25
 Top Global Leaders
 Calendar of Events
 Features
 Company News
 Industry News
 Names in the News
 Products
 RESOURCES
 Archives
 Finishing Today Archives
 Additives Handbook
 Bookstore
 Classified Ads
 Job Search
 Industry Links
 Market Research
 PCI INFO
 Contact Us
 Media Kit
 PCI EVENTS
 Coatings Trends & Technologies
 Powder Coating Forum
 Webinars
Search in: EditorialProductsCompanies
Achieving Six Sigma Objectives for Variability Reduction in Coating Formulation and Processing


November 1, 2001

ARTICLE TOOLS
EmailEmailPrintPrintReprintsReprintsshareShare

Achieving Six Sigma Objectives


Applying design of experiments (DOE) tools can make your coatings system more robust to variations in component levels and processing factors. This is the third article in a series on DOE.1,2

"Six sigma" is the new rallying cry for quality improvement in the chemical process industry. For example, Dow aims to generate an extra $1.5 billion per year in profits after training 50,000 of its employees on the methods of six sigma.3 Statistical tools play a key role in achieving savings of this magnitude. In fact, "sigma" is a Greek letter that statisticians use as a symbol for standard deviation -- a measure of variability. If a manufacturer achieves a six-sigma buffer from its nearest specification, they will experience only 3.4 off-grades per million lots. This translates to better than 99.99966% of product being in specification. To illustrate what this level of performance entails, imagine playing 100 rounds of golf a year: At six sigma you'd miss only 1 putt every 163 years!4

Of all the statistical tools used within six sigma, design of experiments (DOE) offers the most power for making breakthroughs. By way of a case-study example, this article demonstrates how DOE can be applied to development of a coatings system to achieve optimal performance with minimum variability, thus meeting the objectives of six sigma programs.



Minimizing Propagation of Error (POE) from Varying Inputs

Figure 1
Figure 1: Propagation of Error Transmitted from Control Factor X1 (Non-Linear Response)


After earning his Ph.D. in chemistry and taking a job at a chemical company, a colleague of ours got assigned to an operator for an orientation to the real-world of production. As the operator watched with much amusement and disgust, the chemist carefully weighed out materials with a small scoop. The operator pushed the Ph.D. chemist aside, grabbed a sack of chemicals and tossed it into the reactor. "You're not in the laboratory anymore," he said, "This is how we do things in manufacturing."

Hopefully the operators of your coatings systems will be more exacting when adding ingredients. However, at the very least, you can expect some variation due to inherent limitations in equipment. How will these variations affect product quality and process efficiency? Can you do anything to make your system more robust to variations in component levels and process settings? The answers to these questions can be supplied by way of an advanced form of DOE called "response surface methods" (RSM). This statistical tool produces maps of product and product performance, similar to topographical displays of elevation, as a function of the input variables that you (or your clients) control. The objective of six sigma is to "find the flats" -- the high plateaus of product quality and process efficiency that do not get affected much by variations in component levels or factor settings. You can find these desirable operating regions visually, by looking over the 3-D renderings of response surfaces, or more precisely by way of a mathematical procedure called "propagation of error" (POE).



Figure 2
Figure 2: Response Surface Graph of POE Transmitted from Control Factor X1


To see how POE works, let's look at a very simple response surface (see Figure 1) generated by changing only one control factor X1.

Assume that this factor exhibits a constant variation shown on the graph as a difference with magnitude delta (D). This variation, or error, will be transmitted to the measured response to differing degrees depending on the shape of the curve at any particular setting. In this example, because the curve flattens out as the control factor increases, a setting at the higher level causes less POE. Therefore, you see a narrower difference (DY) on the response axis as a result of setting the factor at the higher, rather than lower, level.

With the aid of some calculus, the POE itself can be graphed as a continuous function. In this case the original response surface can be described by the following quadratic equation.



Figure 3
Figure 3: Propagation of Error Transmitted from Control Factor X2 (Linear Response)


We will spare you the details, but after taking the partial derivative of this function with respect to the input (X1) and taking the square root, the following equation for standard deviation (s) is produced.


Figure 4
Figure 4: Achieving Variability Reduction by Intelligent Manipulation of Factor Levels


Assume for now that the standard deviation of the control factor X1 equals one (sx = 1) and there are no other sources of variance (sResidual = 0). We've now obtained the information needed for graphing the standard deviation of the response (sy) transmitted from the variation in the input factor (X) -- in other words, the POE (see Figure 2). In this case the POE decreases in direct proportion to X1 as it increases.

Obviously, reducing response variation is a highly desirable outcome. But what if the absolute level of response gets shifted out of specification? Ideally, you will find another control factor that affects response in a linear fashion, such as that shown in Figure 3. (We added the bell-shaped curves to indicate that variation will likely be distributed according to a normal distribution.)



Figure 5
Figure 5: Therabath Paraffin Therapy Bath


This factor (X2) creates no effect on POE (it's constant), so it can be used to get your response back into specification after changing the other factor (X1) to reduce variability. In this case X2 must be decreased to counteract the increase in response caused by increasing X1 (done to reduce POE). Ideally, as in this simplified example, you can achieve the 'best of both worlds,' as shown in Figure 4: On-target response with minimal variability, hopefully to the level demanded by six sigma.

Let's see how these concepts can be applied to a six-sigma project on a coatings system.



A Case Study on POE:
Powder Coating a Metal Part


Figure 6a
Figure 6a: Effect of Powder Coating Components on Adhesion with Bake Time and Temperature at Mid-Levels


The Therabath paraffin therapy bath5 is a durable medical device that holds one gallon of molten paraffin wax. Sufferers of osteoarthritis use it for physical therapy. They dip their hands repeatedly in the heated bath, which helps loosen stiff joints. The wax then slowly solidifies as a glove, producing further therapeutic benefits through the heat of fusion. Oils reduce the overall melt point to a comfortable level, facilitate removal of the glove and provide moisturizing for skin.

The tank holding the molten wax is made out of stamped steel. It's then powder coated electrostatically with an epoxy-based paint. The coating must withstand temperatures approaching 130 degF. and exposure to salt-water that collects from the sweat of the Therabath users.

The units are sold with a life-time guarantee. Very few units get returned, but in those that do, two types of off-grade predominate.

  • Blisters that appear spontaneously after some time in use
  • Scratches that become noticeably corroded.
It's believed that if adhesion can be maintained at a level above 200, with hardness set at 140, the problems noted above will recede to a level of quality consistent with six sigma. (For reasons of propriety, we do not show units of measure of these responses.)


Designing An Experiment That Combines Mixture with Process Variables

Figure 6b
Figure 6b: / Effect of Powder Coating Components on Hardness with Bake Time and Temperature at Mid-Levels


Our design of experiments combined variations in mixture components and process factors. (See our previous article1 for details on "crossed" designs like this.) Table 1 shows the names and ranges of the input variables, as well as their expected variation in terms of standard deviation, which will come into play when calculating POE.

The mixture variables (A, B and C) were added to a constant of 90 weight % of the powder. The other 10% was made up of bisphenol A, aluminum oxide and silica, all held in constant proportion. The paint chemists expected the three main powder-coating components to interact in complex ways. To properly model such behavior, we wanted to formulate a sufficient number of unique blends to fit a "special cubic" mixture model:



Figure 7a
Figure 7a: Effect of Process Factors on Adhesion with the Powder Coating Formulated at Mid-Levels (centroid)


The process factors of bake time and temperature (D and E) also were expected to interact with each other and possibly create non-linear responses. For this reason, we decided to collect sufficient data for fitting a "quadratic" process model:


Figure 7b
Figure 7b: Effect of Process Factors on Hardness with the Powder Coating Formulated at Mid-Levels (centroid)


Models like this are typically used to develop response surface graphs for process optimization.

These two models were crossed to account for possible interactions between mixture and process. For example, the ideal coating formulation may differ depending on the choice of bake time and temperature, which could be a function of the particular type oven available for processing the tanks. The crossed model contains 42 terms (7 from the special cubic mixture model multiplied by 6 from the quadratic process model). With the aid of computer software,6 a d-optimal design (described in a previous article2) was generated to provide the ideal combinations of variables for fitting response data to the combined mixture-process model. We added five extra unique points for estimating lack-of-fit for the model, plus five replicates of existing points to estimate pure error. We also incorporated one center point (combination #3 on the list), representing the standard operating conditions, for a grand total of 53 combinations.

The results (simulated) of this experiment can be seen in the Appendix. The combinations are organized for easier viewing, with replicate points lumped together. However, experiments like this should always be performed as randomly as possible to offset any lurking variables, such as ambient humidity.



Generating 3D Surfaces to See Impact of Inputs on Responses and POE

Figure 8
Figure 8: Effect of Process Factors on POE of Hardness


Without computer software to do the number-crunching, it would be incredibly difficult to fit all the coefficients in the mixture-process crossed models. It's very cumbersome to even sort through all the statistics generated by such software. We advise that you make use of computerized tools for reducing models to their bare essentials. Make sure that the results pass your pre-set thresholds for statistical significance (typically 95% confidence) and that you don't violate any of the standard assumptions for normality (diagnostic plots help you check this). In this case, the statistical analysis produced highly significant models that met all assumptions. To assess the outcome of an experiment like this, one picture is worth a thousand numbers, so let's not get bogged down in the statistics. Instead, take a look at the response surfaces for the mixture variables (see Figure 6a and 6b) and the process factors (see Figure 7a and 7b) for adhesion and hardness.


Figure 9
Figure 9: Sweet Spots for Processing Powder Coat Made by Optimal Formulation


Notice on Figure 7b how the hardness response drops precipitously at the low ends of bake time and temperature. Even assuming you'd accept such a low hardness, this would be a very bad place to set up your process, because results would be very sensitive to variations in the input factors. This can be seen more clearly in the computer-generated graph of POE shown in Figure 8.


Figure 10
Figure 10: Response Surface for Adhesion as a Function of Bake Time and Temperature with Optimal Formulation of Powder Coat


The highest POE (most variation in response) occurs at the low ends of bake time and temperature. However, before worrying about POE, the system must be set up in a way that meets the basic specifications. Then, assuming that there's optional combinations of input variables that accomplish this mission, pick the one that creates the least POE. This requires use of computer software that can do multiple response optimization.


Finding a Setup that Meets All Specifications with Minimum POE

Table 1
Table 1: Input Variables for Powder Coating Study


As noted earlier, the goals for the Therabath powder-coating properties are an adhesion of at least 200 and a hardness of 140, achieved on a consistent basis by minimizing POE. Furthermore, it would be nice for bake time to be minimized, thus increasing throughput. Obviously, to accomplish all this, some tradeoffs must be made. Therefore, it's necessary to allow for some ranges on all of these goals. Table 2 shows what the Therabath engineers are willing to accept.

The input variables aren't listed in the table, but they do get constrained within their previously specified ranges. Never extrapolate outside of your experimental region because the predictive models probably won't work out there. Stay in bounds or possibly face some dangerous consequences!



Table 2
Table 2: Goals for Powder Coating Study


Based on the goals and ranges, the software set up desirability scales on all responses and then searched for a solution that maximized overall desirability. (For an enlightening discussion on how desirability gets calculated and applied, see reference 7, reprints of which can be obtained by contacting the authors.) The optimal combination found by the software can be seen in Table 3.

Two "sweet spots" can be seen in the process space (bake temperature versus bake time) by overlaying contour plots for hardness and adhesion, with unacceptable regions shaded out (see Figure 9). (The formulation of the powder-coat is set at the optimal component levels shown in Table 3.)



Table 3
Table 3: Optimal Combinations for Mixing and Baking Powder Coat


In this view of the multivariable experimental space, adhesion appears to be more of a limiting response than hardness (it forms most of the boundary around the operating windows at top and bottom). It's tempting to consider reducing the bake time from the recommended level of approximately 26.9 (flag set at starred point in the upper window) to it's minimum tested value of 15 minutes (see flag in lower window). However, as you can see in Figure 10, the adhesion varies the least in the mid-range of bake time (the trough on the response surface).


At the values of 15 minutes for bake time at 364 deg (approximately what's shown in the lower flag in Figure 9) the POE of adhesion exceeds 23 units of standard deviation, a substantial increase from the 18.9 result reported in Table 3 for the optimum setup. In companies that place an emphasis on six-sigma goals this may be an unacceptable trade-off. However, if time is of the essence, it's easy enough to incorporate this in the optimization criteria - simply add a goal to minimize it. That's what makes the whole DOE procedure outlined in this article so incredibly powerful: It produces statistically valid predictive models that can be easily manipulated for "what-if" analysis. Then when goals shift, or get weighted differently, it's just a matter of plug-and-chug and the answer magically appears. To ensure that it's correct, confirmation runs must be performed. Hopefully, the results will agree well with what's predicted to happen.


Conclusion

As a result of doing systematic experimentation, using sound statistical principles, the quality of the powder-coating of Therabath tanks can be improved and became more robust to variations in the levels of components and processing factors. With the proper knowledge and software tools, coatings chemists and engineers can apply these same methods to their systems and accomplish similar breakthrough improvements.

For more information on design of experiments, contact Stat-Ease Inc., 2021 East Hennepin Ave., Suite 191, Minneapolis, MN 55413; phone 612/378.9449; fax 612/378.2152; e-mail Mark@StatEase.com; or Circle Number 80.



References

1 Anderson, M.J.; Whitcomb, P.J. "Design Experiments that Combine Mixture Components with Process Factors," PCI November 2000.
2 Anderson, M.J.; Whitcomb, P.J. "Computer-Aided Tools for Optimal Mixture Design," PCI, November 1999.
3 "Making Six Sigma Benefits Stick," Chemical Week Vol. 163, No. 19. p. 40, 5/9/2001.
4 Phelan, S. "Six Sigma, "Information Technology & You: Creating A Happy Customer," PCI, website http://www.pcimag.com/pci/cda/articleinformation/features/bnp__features__item/0,1846,388,00.html
5 WR Medical Electronics Co., 123 N. 2nd St., Stillwater, MN 55082.
6 Helseth, et al, Design-Expert, Version 6 for Windows, Stat-Ease Inc., Minneapolis, 2001.
7 Anderson, M.J.; Whitcomb, P.J. "Optimization of Paint Formulations Made Easy with Computer-Aided Design of Experiments for Mixtures," J. Coatings Technol., Volume 68, Number 858, July 1996, pages 71-75.


|PrintEmail

Did you enjoy this article? Click here to subscribe to the magazine.

BNP Media
© 2010 BNP Media. All rights reserved. | Privacy Policy