Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Polyester Polyols Based on Polymerized Fatty Acids From Renewable Resources

By Erwin Honcoop, William NcNamee
September 1, 2009

High-performance materials such as solventborne coatings have been produced from polyurethanes for many years. However, with current regulatory pressures, a move to water systems and to materials from bio-based renewable resources is necessary. Although it is possible to formulate waterborne polyurethane systems, the widely used adipate polyester backbones often cause problems, such as reduction in storage stability and hydrolytic resistance. Additionally, the water evaporation rate of polyurethane dispersions is seen as a drawback in certain applications such as UV-curable coatings and adhesives.

However, a range of hydrolytically stable polyester polyols using bio-based technology has overcome these deficiencies. The reduced number of ester bonds and the hydrophobic environment make these polyols practically immune to water, while maintaining thermal- and UV-resistance characteristics.

In this paper, it is demonstrated that these polyester polyols, produced from C-36 dimer fatty acids, improve the hydrolytic and storage stability of polyurethane dispersions. Additionally, results will show that UV-curable polyurethane dispersions produced from these polyols exhibit these same properties, as well as significant improvement in water evaporation that leads to improved cure time.

Finally it will be demonstrated that the adhesion properties of coatings on different plastic substrates improve considerably.

Dimer Fatty Acids

Natural oils and fats have for years provided the polyurethane chemist with a variety of building blocks, such as glycerine and castor oil. Less well known is the use in polyurethane chemistry of a fatty acid derivative, the so-called dimerized fatty acids. These are obtained by the conversion of unsaturated fatty acids (from sources like soybean oil or tall oil) by a combination of pressure, temperature and catalysis. This process generates a mixture of products, the most important being dimerized fatty acid. Others are trimerized fatty acid, and isostearic acid (Figure 1).

Starting from the C-18 acids that nature typically provides, the dimer acid is a molecule with 36 carbon atoms, which makes it by far the longest dioic acid available. This hydrocarbon nature makes the dimer acid and polymers in which it is included extremely hydrophobic. In addition, the combination of hydrocarbon character and non-crystallinity provides lubricity and flexibility, even at very low temperatures.

Dimerized fatty acids have found their application in areas such as polyurethane, UV-curable and polyester coatings, both solvent and waterborne systems. In all these applications, the value of the dimerized fatty acid is related to the features mentioned: flexibility and impact strength, wetting and flowability, and hydrophobicity and hydrolytic resistance.

Polyurethane Dispersion Based on Dimer Technology

The dimer fatty acids provide polyester and polyurethane coatings with a range of favorable features, such as flexibility and hydrolytic resistance. Clearly, other coating systems could benefit from the introduction of dimer acids as well. Conversion of dimerized fatty acid to the corresponding diol, or by building dimerized fatty acid into hydroxyl-terminated polyesters, makes it suitable for incorporation in polyurethanes (Figure 2). The dimer fatty acid-based polyester polyols can be semi-crystalline or amorphous type, depending on the choice of polyol monomer.

When comparing polyurethanes based on dimerate poly­esters to adipate polyesters, polycaprolactone polyols and polyether polyols, it becomes clear that they form a category of their own. Compared to the adipates, the dimerates exhibit much lower moisture absorption, lower hydrolysis rate, and greater flexibility. In comparison with polyethers such as polyethylene glycol (PEG), polypropylene glycol (PPG), or polytetramethylene glycol (PTMEG), the absence of ether linkages makes dimer-based polyurethanes much more resistant to degradation by radical-type attack, such as heat, oxidation or ultraviolet radiation.

This combination of stability against both hydrolysis and radical-type attack is unique, and is highly relevant for applications like heavy-duty coatings and adhesives, and automotive elastomers. Additionally, it has been found that dimer technology brings low-temperature flexibility, flowability and affinity for low-energy surfaces. No monomer comes closer in composition to a polyolefin than dimer acid.

A range of dimer-based polyester polyols is commercially available, and these materials have been tested in polyurethane dispersions. The fact that dimer fatty acids are hydrophobic makes it challenging to disperse them in water, but this can be resolved by using the correct addition method during processing.

The polyurethane dispersions based on the dimer acid technology exhibit mechanical strength, adhesion, grain enhancement, gloss and chemical resistance. Especially noticeable is the improved resistance to water when compared to adipate-based polyester polyols. The dimer fatty acid-based polyol shows no damage to the surface, where the adipate shows severe damage after hydrolytic exposure to the surface.



Additionally, the water uptake of the polyurethane films has been evaluated. In Figure 3, one can clearly see that the hydrophobic character of the dimer fatty acid has a positive impact on water uptake. The adipate-based polyurethane film absorbs up to 8% water at 23 °C and the PTMEG-based films even up to 10% versus only 1-2% for dimer fatty acid-based polyols.





Hydrolytic Resistance

One of the challenges of water-based systems is the hydrolytic stability on storage. This is especially the case when polyester polyols are incorporated within the backbone of the polyurethane. Several polyurethane dispersions were exposed to storage at 50 °C after which the retention of the film strength was re-evaluated. Figure 5 shows that inclusion of dimer fatty acid-based polyester polyols in the backbone significantly improves the storage stability over an adipate-based polyester polyol. This can be explained through the hydrophobic nature of the dimer-based polyester polyols, protecting the ester-bonds from hydrolysis.

UV-Curable Polyurethane Dispersion

As demonstrated, polyurethanes based on dimer-based polyester polyols exhibit significantly improved hydrolytic stability and weatherability. These improvements are also relevant to the UV polyurethane dispersions.

UV-polyurethane dispersions were prepared using the prepolymer process route in which the addition reaction between the dimer-based polyester polyols, dimethylolpropionic acid and isocyanates takes place in the presence of water-dilutable solvents such as ethyl acetate. The formation of the prepolymer takes place in the organic phase and after the theoretical NCO content has been reached, the prepolymer is further reacted with pentaerythrytol triacrylate. Before transferring the polymer into the water, the carboxyl groups are neutralized with a tertiary amine. Once successfully dispersed into water, the low-boiling solvent is removed by gentle distillation, to give a solvent-free UV polyurethane dispersion with a solids content of approximately 35%.

For this study polyols with a Mw of 2000 were used. These were hexanediol adipate, PTMEG-diol, a semi-crystalline dimerate and an amorphous dimerate. The coatings were cured using 4 passes 80 Watt/cm at a speed of 15 m/min for the evaluation of the chemical and mechanical resistance at a thickness of 50 µ dry coating.

A major disadvantage of UV-PUDs is that an additional step of drying is required to remove the water from the system. Keeping in mind the hydrophobic nature of the dimer fatty acid-based polyester polyols and the need to evaporate the water before UV curing, the influence of the hydrophobic dimer-based polyols was screened.

For this we looked at a drying cycle used in the industry when UV-PUDs are applied. As can be seen in Figure 6 the drying step in the oven for the water evaporation is a time-consuming step. If one could increase the evaporation rate of the water, this time could be shortened. The UV-PUDs prepared in this study were evaluated on the loss of water during the drying. For this a thermographic analyses was used, using the same weight and solid content of the dispersions. IR-drying was used for the oven, at a temperature set at 60 °C. The results in Figure 7 show that both polyesters containing dimer fatty acid exhibit a definite advantage in terms of faster water evaporation over the adipate ester and the polyether.

Adhesion Properties

The adhesion properties of the polyurethane dispersions were evaluated, not using normal coating adhesion test methods but a method used in the adhesive industry. This has been done to distinguish in an alternative way the adhesive strength of the PU dispersions. The method used is a lap shear adhesion test, where the polyurethane dispersions were tested on several plastic substrates.



The adhesion of uncrosslinked PU dispersion is highly improved upon addition of dimer into the polyol. For crosslinked PU dispersions, the adhesion is comparable for all PU dispersions.

The PU dispersion based on the adipate polyol gives a low adhesion to tested substrates and fails almost immediately. Dimer improves the adhesion significantly, probably due to the increased flexibility of the coating, resulting in increased stress absorption. The test results are shown in Figure 8.

Conclusion

It has been demonstrated that the polyester polyols based on dimerized fatty acids offer several unique properties to polyurethane dispersions. The hydrophobic nature of these products significantly improves the hydrolytic stability of the polyurethane dispersions and, therefore, improves the storage stability of these products. The same hydrophobic properties also enhance the evaporation rate of the water during the drying cycle of UV- polyurethane dispersion systems.

Furthermore, the morphology of the dimer fatty acid structure within the polyester polyol leads to significant improvement in the adhesion on plastic substrates such as PET, ABS and PE in comparison with adipate-based polyols.

Polyester polyols based on dimer fatty acids from renewable bio-based resources form a class of versatile raw materials for polyurethane dispersions that allow the resin producer to overcome some of the major challenges of this technology.

This paper was presented at the Waterborne Symposium sponsored by The University of Southern Mississippi School of Polymers and High Performance Materials and The Southern Society for Coatings Technology, 2009, New Orleans, LA.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Erwin Honcoop, Croda, Gouda, NL
Croda Incorporated, New Castle, DE

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • Improving Waterborne Alkyd Resins With Fatty Acids

    See More
  • Piedmont Chemical Launches Renewable Polyester Polyols

    See More
  • Polyester Polyols for Water-Resistant Polyurethane Coatings

    See More

Related Products

See More Products
  • biopolymer.jpg

    Biopolymer-Based Films and Coatings Trends and Challenges

  • Optimizing Social Media from a B2B Perspective

See More Products

Related Directories

  • Cargill

    Cargill offers vegetable‑based ingredient solutions for modern coatings. The portfolio includes high‑quality vegetable oils with film‑forming properties, distilled fatty acids for formulation efficiency, and polymerized vegetable oils designed to support durability and application performance.
  • Vertec BioSolvents Inc.

    Sustainable, safe, bio-based performance solvents and blends from renewable resources to replace petroleum-based solvents for formulating, blending and cleaning.
  • Vertec BioSolvents Inc.

    Environmentally friendly, safe, sustainable bio-based performance solvents and blends from renewable resources to replace petroleum-based solvents for formulating, blending and cleaning.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing