Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

2K Waterborne Concrete Floor Coatings

By Karl Sundberg, Ming Tsang
November 1, 2009


Epoxy-based liquid coatings have been used for decades in many heavy-duty applications such as high-end metal primers and industrial flooring paints. Generally, epoxy systems provide many benefits, including excellent adhesion to various substrates such as metal and concrete, as well as outstanding water, chemical, corrosion and abrasion resistance.

Two-pack (2K) epoxy-amine coating systems are commonly used when heat curing is not possible because epoxy groups can readily react (crosslink) with the primary and even secondary amine groups of amine hardeners at ambient temperature. In recent years waterborne, 2K epoxy-based garage concrete floor paints have been gaining popularity among contractors and do-it-yourselfers since they are regarded as more environmentally friendly when compared to their solventborne counterparts.

On the other hand, organic solvents such as various glycol ethers are believed to be used in many waterborne 2K epoxy concrete floor paints to improve: dry time and open time; handling by viscosity reduction of the epoxy resins and hardeners; the dispersion of hydrophobic liquid epoxy resins in aqueous formulas; and film formation and pot life.1

However, due to lowered VOC limits enacted in certain areas, as well as other proposed regulation changes in North America and Europe, there is a need to reduce the VOC of existing paint products. For example, one of the most stringent sets of VOC regulation is Rule 1113 for Architectural Coatings from South Coast Air Quality Management District (SCAQMD); the VOC limit for floor coatings was reduced to 50 g/L as of July 2006.

This study investigates the feasibility of formulating waterborne 2K epoxy concrete topcoats with VOC below 50 g/L, while maintaining the good performance properties offered by existing commercially available but higher-VOC products.

The typical performance requirements of waterborne 2K epoxy concrete paints include: easy to hand-mix parts A and B; pot life of 2 hours or more; good chemical and hot tire resistance; and good adhesion and gloss stability throughout the pot life.

Experimental Materials and Formulations

In this study, several modified epoxy resins (Epoxy X, Epoxy Y and Epoxy Z) were evaluated and benchmarked against a Bisphenol-A-based liquid epoxy resin, Epoxy W. Hardener H, an amine hardener that has been used in waterborne concrete coatings, was chosen in our study to crosslink with the epoxy resins. Characteristics of all these resins are summarized in Table 1. Please note that the epoxy equivalent weight (EEW) and amine hydrogen equivalent weight (HEW) quoted in this table are based on the form of delivery of the materials (as supplied).



Liquid epoxy resins, Epoxy W and Epoxy X, were evaluated in simple clearcoat formulations as shown in Table 2. Note that flow and leveling Additive S is a silicone-based additive containing 50% by weight VOC. It was used to promote proper substrate wetting in these low-VOC formulas.

In addition, two different blends of epoxy resins were evaluated in clearcoat Formulas #7 and #8, as shown in Table 3.

Finally, two pigmented formulas, shown in Table 4, were also evaluated.

Sample Preparation

For gloss measurements, drawdowns of Formulas #1 to #10 were made on coated drawdown cards by using a Bird type 3-mil drawdown applicator. All drawdowns were allowed to dry at room temperature for at least one day.

Concrete panels (blocks) used in this study were made by type 1 cement according to ASTM method D 5139-90, without the use of mold release agent, and aged for at least 30 days. All blocks were acid etched, rinsed and then dried for one day at room temperatures before being used as coating substrates.

For the rest of the performance testing, coated concrete panels were prepared by brushing using a 1” bristle brush. Wet film thickness between 3 to 6 mil was targeted. For adhesion evaluation, 24 h spot test, and hot tire resistance testing, coatings were applied 1 h after the initial mixing of parts A and B (activation). All panels prepared for adhesion evaluation and 24 h spot test were dried and cured at room temperature for at least 7 days.

Performance Testing

Gloss Measurement
Gloss was measured at 60° angles by a hand-held gloss meter (BYK-Gardner brand, model Micro TRI-Gloss).

Adhesion
Crosshatch adhesion on concrete blocks was performed according to ASTM 3359-07, except for the use of 3 mm spacing between cuts. Scotch® brand tape type 898 was used. A rating of “5B” represents 0% of coating detached, while “0B” represents > 65% of the coating detached. A minimum of 4B adhesion was used in this study as our criteria for a ‘pass’ rating.

Chemical Resistance
Chemical resistance was evaluated using 24 h spot test. Testing was performed over concrete panels according to our internal method SOP ST-LC-46, which is similar to ASTM D 1308-02. Reagents were covered with glass during the 24 h testing period, and the spots were evaluated immediately after reagents were removed by wiping.

Hot Tire Resistance
Hot tire resistance test was done according to our internal test method SOP ST-LC-59. Pre-cut 3”x3” tire pieces were clamped to the coated concrete panels at 40 psi pressure with a torque-adjustable wrench, and then heated for 4 h at 40 °C (Figure 1). After heating, the tire pieces were removed immediately and the coatings were observed. A pass rating was given if no coating was removed regardless of tire staining. All coatings were applied 1 h after activation.

Test concrete panels were coated by brushing, and cured at different time periods before testing at:
  • 24 h after coating application;

  • 24 h after application followed by covering with a wet paper towel for 4 h;

  • 72 h after application; and

  • 72 h after application followed by covering with a wet paper towel for 4 h.



Results and Discussion

Comparing Epoxy X with Epoxy W
Since ease of mixing between parts A and B was an important feature, we compared the water miscibility of both liquid epoxy resins, Epoxy X (a modified epoxy resin) and Epoxy W (an unmodified Bis-A based epoxy resin). Each epoxy resin was hand-mixed with equal parts of water without using any organic solvent. It was found that while hydrophobic Epoxy W was immiscible with water, Epoxy X could form a low viscous milky emulsion (Figure 2) without much difficulty. This indicated that Epoxy X had an advantage over Epoxy W in terms of ease of mixing.



Pot life Evaluation Based on Gloss and Adhesion
For Formulas #1 to #6, gloss (Figure 3) and adhesion (Table 5) were measured at various time intervals after activation.

All formulas, from #1 to #6, seemed to provide adequate pot life (> 2 h) based on monitoring the gloss levels after activation. However, only Formula #3, #5 and #6 could maintain adhesion of 4B or more at 2 h after activation. It seemed that adhesion performance would be a better choice to monitor pot life.



Formula #3 contained more than 7% of solvent EP and had a VOC of 150 g/L. This formula was used in this study as an internal “control” for comparison. It had the longest pot life as monitored by adhesion, and it seemed to prove that the use of solvent could indeed improve pot life. However, it was also found that solvent did not always improve performance. For example, when compared to its solvent-free counterpart (Formula #2), Formula #3 showed a drop of gloss sooner (3.5 h) after activation.



On the other hand, Formulas #5 and #6 both had VOC levels below < 50 g/L, and they met both pot life and VOC requirements of this study. When compared to their counterpart, Formula #2, it seemed that by using a stoichiometry ratio HEW:EEW of 1.1:1.0, the pot life as monitored by adhesion could be improved slightly in clearcoat formulations, and a minimum of 2 h pot life was achievable.

Formulas #7 and #8 were evaluated to see if the use of epoxy resin blends would also result in satisfactory pot life while maintaining VOC at < 50 g/L. Figure 4 showed the gloss levels and adhesion of both formulas after activation.

Even though both Formulas #7 and #8 showed pot life of well over 2 h as monitored by gloss, only Formula #7 could maintain a 4B adhesion at 2 h after activation. It showed that by using a proper blend of epoxy resins (Epoxy X and Epoxy Z), pot life of 2 h minimum could also be achieved in clearcoat formulas.



Lastly, Formulas #9 and #10 were evaluated (Figure 5) to see if acceptable pot life could be achieved if the epoxy resins were evaluated in pigment-containing formulas.

Formula #10, made by a blend of epoxy resins (Epoxy X and Epoxy Z) was able to provide a pot life of 3 h after activation, as monitored by both adhesion and gloss. However, Formula #9, which was based on Epoxy X only, failed to achieve the 2 h minimum pot life.

In summary, it was found that by using epoxy blends of Epoxy X and Epoxy Z, low-VOC clearcoats and pigmented coatings could be formulated with a minimum of 2 h pot life.



Chemical and Solvent Resistance
Table 6 shows a result summary of 24 h spot test, which was performed on Formulas #3, #6, #7 and #10. All of these formulas showed acceptable pot life of 2 h minimum.

When compared to Formula #3 (a high-VOC “control”), Formulas #6, #7 and #10 showed very similar chemical resistance results. This test showed that the chemical resistance of both clearcoat and pigmented formulas was not affected by their VOC levels.



Hot Tire Resistance
A summary of hot tire test results of Formulas #3, #6, #7 and #10 are given in Table 7. All of these formulas passed the hot tire resistance tests, under all four different curing/pretreatment conditions. It showed that even though Formulas #6, #7 and #10 had much lower VOC levels comparing to Formula #3, these three coatings were able to develop the necessary hot tire resistance after curing for as little as 24 hrs.

Conclusions

By using specific raw materials (Epoxy X, Epoxy Z and Hardener H), along with proper formulation techniques (such as proper stoichiometric ratios), formulating waterborne 2K epoxy concrete coatings meeting the following requirements is possible:
  • VOC levels of less than 50 g/L;

  • easy to hand-mix parts A & B;

  • pot life of 2 hours or more;

  • good chemical and hot tire resistance; and

  • good adhesion and gloss stability throughout the pot life.



Acknowledgements

The authors want to acknowledge our company’s entire Global Concrete Segment Team, with members among different business functions across Europe and the United States, for their contribution and support in this study.

Note

Formula #7 evaluated = Starting point formula # 1558, Clear concrete topcoat
Formula #10 evaluated = Starting point formula # 1559, Gray concrete topcoat
Both formulas are available from Cytec.


This paper was presented at the American Coatings Conference, 2008, Charlotte, NC.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Cytec Industries, Inc., USA
Cytec Industries, Inc., USA

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Paint and Coating Market Reports
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • Study Sees Growth in Concrete Floor Coatings Market

    See More
  • Magnifying glass and documents with analytics data lying on tablet

    Concrete Floor Coatings Outlook Trends Up

    See More
  • Dutch Boy Paints Introduces a Full Lineup of Concrete and Masonry Floor Coatings.jpg

    Dutch Boy Paints Introduces a Full Lineup of Concrete and Masonry Floor Coatings

    See More

Related Products

See More Products
  • Waterborne Polymers and Film Formation (Virtual Course - 7/23/26)

See More Products

Events

View AllSubmit An Event
  • March 31, 2026

    Durability by Design: Waterborne Concrete Coatings that Protect, Beautify, and Extend Service Life

    On Demand Attend this webinar to understand how protecting concrete enables lifespan extension and reduction of the CO₂ emissions associated with premature repair or replacement.
View AllSubmit An Event

Related Directories

  • EIT2.0 LLC

    EIT2.0 designs, manufactures, sells and supports UV radiometers, UV profiling radiometers and online sensors for UV LED, arc, microwave and spot sources. EIT2.0 products and support are available worldwide.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing