Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!
FT Archives

Artificial vs. Natural Testing

By Henry K. Hardcastle
August 4, 2006
A recent study is helping to improve the connection between laboratory and outdoor testing, thereby enhancing material service life predictions.



Figure 1. Two variable model functions from the xenon arc trials.

Predicting material service life is an important aspect of any quality analysis operation. However, for materials that are intended for use outdoors, developing such a prediction can be challenging. Outdoor reference laboratory exposure testing can take years to complete, significantly delaying the introduction of new products to the market. In many cases, a more desirable alternative is accelerated laboratory testing using artificial weathering devices. But can such devices accurately predict the service life of a material exposed to outdoor weather?

Researchers at Atlas Material Testing Technology LLC recently performed a study to help identify gaps in their understanding of applying Arrhenius models developed in artificial weathering devices to outdoor reference environment exposures and ultimately to predict material service life at locations throughout the world. The study used the yellowing of unprotected polycarbonate as the measured variable for assessing service life according to ASTM E 313-96 for 2°/C.1 A yellowness index (Y.I.) change of 6 units was arbitrarily identified as the end of useful service life for this study.

The study involved two main parts: developing an Arrhenius weathering model in artificial xenon arc exposures, and verifying the model in outdoor reference exposures. The three input variables considered by the Arrhenius model included ultraviolet (UV) light intensity, standard black panel temperature (BPT), and percent relative humidity (R.H.%). A large supply of commercially available unprotected polycarbonate was obtained, cut into 2 x 6-in. specimens and randomized. Samples of specimens were then exposed in xenon arc weather testing instrument exposures and outdoor reference laboratory exposures in Miami, FL and Phoenix, AZ. The outdoor exposures were started years before the xenon arc weather testing instrument exposures.

Artificial Laboratory Weathering

The purpose of the artificial laboratory weathering trials was to understand considerations for developing Arrhenius type service life prediction models using xenon arc exposure devices. Artificial laboratory exposures were conducted in Atlas model Ci5000 and Ci4000 Weather-Ometers® with no spray and no dark cycles. The exposures used a quartz inner/borosilicate outer filter combination. Irradiance levels, BPT and R.H.% levels were adjusted to a variety of levels for seven trials in this study.

The xenon exposure used seven trials with 10 polycarbonate specimens for each trial and input variables as specified in Table 1. At convenient intervals, technicians paused the exposure and removed the specimens to measure Y.I., followed by continued exposure. Trials used shorter exposures and less frequent measurements as the study progressed since the material's degradation function appeared linear with the UV radiant exposure throughout all trials. For each specimen in each exposure, an equation for best-fit line was determined relating the change in Y.I. to the UV exposure in KJ/m^2·nm at 340 nm. These equations were then used to predict the amount of UV exposure to produce a delta Y.I. of 6 for each specimen under each exposure condition. The average prediction for each xenon arc exposure trial condition is shown in Table 1.

Once the xenon arc exposure data for each input variable combination was obtained, the next step converted input variables into an appropriate form for the Arrhenius relationship: Ln (life estimate in KJ/m^2·nm at 340 nm), UV radiant intensity in W/m^2·nm at 340 nm, 1/°K BPT, and R.H.%. The exposure input variables and dependent variable (Ln [life estimate]) were entered into a standard statistical analysis software package (Statistica 6 by StatSoft, Inc.). Simple multiple linear regression analysis was performed on the 73 data points.2 The results of this analysis are shown in Table 2. From this analysis, technicians obtained a predictive model describing the polycarbonate yellowing weathering behavior in xenon arc exposure as a function of UV irradiation level, BPT and R.H.%. Figure 1 shows the model function for two of the three variables, as well as observed data. The observed data showed reasonable agreement with predicted data from the regression model.

Outdoor Reference Weathering

The purpose of the outdoor reference environment weathering was to expose the same polycarbonate material to real, variable outdoor weather while carefully measuring the variables that were controlled in the xenon arc exposure trials. The intent was to see whether the Arrhenius model could use measured levels of UV light intensity, BPT and R.H.% obtained outdoors for a prediction of service life that was in reasonable agreement with observed service life. By performing outdoor exposure of the polycarbonate material at the reference exposure laboratories, technicians obtained frequent measurements of UV light intensity, BPT and R.H.% at the same location as the material's outdoor exposure.

Five independent exposures of the polycarbonate material were performed in Miami and Phoenix at Atlas Weathering Services exposure facilities. All exposures were conducted at an angle of 5° facing south in an unbacked configuration. The five exposures started on different years and at different seasons of the year at the different locations. The change in Y.I. as a function of total UV exposure for the different tests is shown in Figure 2 (p. 42). Technicians observed the service life of the polycarbonate as approximately 380 and 450 MJ/m^2 total ultraviolet radiation (TUVR) in Miami and Phoenix, respectively, for these exposures.

Materials were exposed within 0.5 km of radiometric, BPT and R.H.% measurement devices. TUVR, BPT and R.H.% data was obtained for the years 2000 and 2003 at 30 minute intervals throughout each day of the year at these locations. Technicians constructed an average year from these data points. An example of this 30-minute average data for a single summer day in Miami is shown in Figure 3.

Figure 2. Example of single day black panel temperatures and irradiance values in Florida exposure.

Linking Laboratory and Outdoor Data

Using the Arrhenius model developed in the xenon arc exposure trials to predict outdoor weathering conceptually involves a simple process of measuring the input variables observed in the outdoor environment, putting these values into the model and calculating the function for these outdoor variable levels. In this study, technicians performed exposures and variable measurements at the same exposure locations to allow for a close comparison between predicted results from the model with observed results from the outdoor exposures. Currently, this process appears to be one of the largest sources of error in applying the developed models because very considerable differences exist between the variable measurements of the xenon arc weather testing instrument compared with the variable measurements of the outdoor reference exposures.

The task of inputting the 30 minute outdoor UV light intensity, BPT and R.H.% data into the Arrhenius model proved highly problematic. In the xenon arc exposures, the light intensity variable is measured in W/m^2·nm at 340 nm. In the outdoor exposure, the light intensity is measured in W/m^2·nm from 295 to 385 nm. Optimally, both the model-measured variables and the outdoor-measured variables should be measured in the same way, with devices of identical response. However, this replication of variable measurement did not exist for this study.

To obtain comparable data, technicians used a proportional approximation of UV light intensity. Sources reported that a reasonable average maximum noontime light intensity value in Miami was about 0.65 W/m^2·nm at 340 nm. Observing that the TUVR data (295-385 nm) light intensity level was about 0.065 for noontime summer in Miami, the technicians simply multiplied the observed TUVR data by 10 to obtain a proportional approximation for 340 nm W/m^2·nm light intensity. Although a very rough, crude approximation, the predicted reference environment exposure data for polycarbonate was within reasonable agreement with the observed exposure data.*

Black panel temperature measurement devices used in the outdoor reference environment differ significantly from the black panels used in the xenon arc instrument chamber. Different black coatings, metallic substrates and temperature measurement sensors may result in different temperature measurements. The technicians also did not have data correlating xenon arc BPTs to outdoor BPTs, and therefore could not apply a suitable conversion factor. Instead, they used the outdoor BPT data as an input into the Arrhenius model developed with the testing instrument BPT input. Although this represents an obvious offset in the BPT model variable and sources of error in the estimated life calculation, the predicted reference environment exposure data appeared in reasonable agreement with the observed exposure data.

Figure 3. Observed reference exposure results compared to predicted model results.

Observed vs. Predicted Results

To use the Arrhenius model developed with the xenon arc exposures, technicians took the 30 minute outdoor variable data (calculated as explained previously), entered the UV light intensity approximation, BPT and R.H.% value for each 30 minute interval into the Arrhenius calculation, and obtained a value for expected degradation for that 30 minute period. All data points for which the light intensity was zero (nighttime) were disregarded, and all the individual values for the duration of the exposures were summed. The model predicted estimates for service life are compared to the actual observed values in Figure 3. In both exposure environments, the predicted service life estimate differed from the observed service life by less than 15%. Given the differences in variable measurement and the crude approximations undertaken in the calculation, this level of agreement was unexpected for a first approximation.

Ensuring Accurate Predictions

Accelerated laboratory testing using artificial weathering devices is not an exact substitute for natural outdoor testing. However, advances are continuously being made in the accuracy of such instruments through studies such as the one described in this article. As a result, today's artificial weathering devices can be used to reliably predict service life with a small margin of error. Further reliability is gained by combining accelerated laboratory testing with natural outdoor testing to allow for a more detailed survey of the various processes occurring at the molecular level.

Author's note: The information presented in this article is not meant to address the service life prediction of polycarbonate but only to investigate considerations for applying service life prediction methodologies to exposure data. Further, this study is only presented to highlight some considerations for performing these types of service life prediction methodologies, and use of this information for any other purpose is not recommended.

*Atlas Material Testing Technology does not recommend use of this approximation for anything outside this project. Service life prediction efforts should use actual measured values used in determining the predictive models.

SIDEBAR:
Artificial Reference Exposure Comparison Considerations

Future service life prediction (SLP) investigations may benefit from several specific considerations noted during this study:
  • SLP efforts should provide for identical exposure variable measurements in the xenon arc exposures, at the outdoor reference exposure locations and at the worldwide exposure locations.
  • The UV light intensity measurements in the xenon arc chambers should be duplicated in the outdoor exposures.
  • The BPT measurements in the xenon arc chambers should be duplicated in the outdoor exposures.
  • Further studies should consider actual material surface temperature measurements rather than BPT data for use in predictive models.
  • The methods and frequencies for measuring environmental variables should be standardized throughout outdoor reference exposure laboratories and worldwide exposure locations.
  • Future SLP investigations should consider using virtual environmental variable data (as generated from weather modeling software), as well as actual measured environmental variable data to compare differences with observed exposure service life and life estimates from modeled weather variables.
  • Models developed from xenon arc exposures using Arrhenius approaches yielded first approximations with reasonable agreement to outdoor observed values, while regression models without Arrhenius concepts appeared very limited for outdoor predictions in this study.
  • It may be possible to perform correlation studies to obtain conversion factors for W/m^2_nm at 340 nm to TUVR MJ/m^2 in order to enhance first approximations.
  • Both the two-variable (UV intensity and BPT) and three-variable models (UV intensity, BPT and R.H.%) explained most of the variation observed in the xenon arc trials of this study.
  • The xenon arc air chamber temperature variable did not contribute significantly to the predictive model developed in this study.
  • The frequent environmental data logging from the reference exposure locations (30 minute intervals) appeared sufficiently frequent for the first approximations of this study.
  • It appears highly desirable to obtain worldwide exposure durations expressed as UV exposure rather than as months time duration.
  • The averaging and approximation techniques used for putting environmental variable data into predictive models, although undesirable, appeared effective for the first approximations of this study
  • It appeared important to disregard nighttime data in the predictive calculations.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Henry K. (Kelly) Hardcastle is director of Research and Development for Atlas MTT LLC Weathering Services and is responsible for designing, analyzing and presenting experiments involving durability of materials. He has 18 years of experience in weathering and materials degradation on an R&D and quality assurance level. For more information, call 773-327-4520, e-mail info@atlas-mts.com or visit www.atlas-mts.com.

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • Dow Polyurethanes Successfully Completes Testing Phase for Natural Oil Polyols

    See More
  • Dow Polyurethanes Completes Testing Phase for Natural Oil Polyols

    See More
  • The Paint and Coatings Industry vs. Commoditization

    The Paint and Coatings Industry vs. Commoditization

    See More

Related Directories

  • Atlas Material Testing Technology LLC

    For more than 100 years, Atlas has been a leader in materials testing, offering a complete line of weathering testing instrumentation, laboratory, and outdoor testing services.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing