Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

"Green" UV Coatings Technology Comes to Total Door

By Dan Sweetwood, Michael Kelly, Kevin H. Joesel
May 1, 2010
This company implemented  UV coatings technology to replace a solvent-based system to increase production capabilities and provide a safer work environment for employees.



“In a time of unprecedented economic uncertainty, we have been able to strategically position ourselves to meet the current and future needs of our customers.” Those were the words stated by Patricia Yulkowski, Total Door® Chief Executive Officer, marking the grand opening of Total Door’s new environmentally conscious, Feng Shui-inspired, innovative manufacturing and training facility.

What may not have been touted as loudly as the significant historical event of the grand opening are the impressive “green” innovative processes, materials and tools that Total Door has designed into its manufacturing system. Patricia Yulkowski notes that “80% of our material is recycled, and we have significantly reduced the use of volatile organic compounds. Our door systems are also made in the United States, whereas 80% of builder’s hardware product is manufactured overseas.”

An exceptional example of one of Total Door’s innovative process changes was moving from solvent-based coating to UV coating technology. The move was a major part of the company’s green strategy, and teaming with Allied PhotoChemical, Inc., a Michigan-based UV technology company, delivered the right solution – streamlining the manufacturing process, for Total Door’s needs.

Total Door’s decision to move from solvent-based coating to UV coating technology was based on “sustainability” of the technology. UV coating provides a platform for Total Door’s manufacturing based on the following key attributes:
  • faster production speed;

  • reduced work in process;

  • reduced manufacturing footprint;

  • reduced energy costs;

  • reduced quality costs;

  • cleaner – no VOCs or HAPs; and

  • cleaner and safer work environment.

Sustainable UV coating technology offers a process that has many benefits that deliver to the bottom line for Total Door. This technology enables the company to run its door manufacturing process at a higher line speed, which offers them more production capacity and flexibility. In addition, the UV coating process offers a cure time of less than two seconds, which offers many benefits, from immediate handling to reduction in quality costs. Also, UV coatings are typically 100% solids, meaning no solvent or water content to deal with – a much greener process.

From a production standpoint, UV coating technology offers Total Door the ability to implement a process that consumes a great deal less floor space, mainly by reducing or eliminating conventional ovens and conveyors. “Work in Process” is virtually eliminated due to the instant cure properties of the UV coating process. With these reductions, energy costs are also reduced. One main area of focus for Total Door is overall quality and the costs associated with quality. The ability to immediately inspect UV-coated cured parts is critical to Total Door’s goal to continually reduce quality defects. The UV paint process delivers this capability.

The sustainability of UV coating technology offers Total Door a means to greatly reduce its VOC emissions, as most UV coatings contain no VOCs or HAPs (Hazardous Air Pollutants). Typically, UV coatings offer the manufacturer reduced reporting as well as cleaner and safer work environments.

Total Door Manufacturing Flow

Figure 1 outlines the details of the UV coating process at Total Door. The system has two bell atomizers that are reciprocated. The coating is applied electrostatically, ensuring excellent coating coverage.

After the coating is applied, two Fusion microwave UV lights are reciprocated on each side of the product. This ensures that adequate curing of the coating takes place. Figure 1 is a pictorial representation of the UV coating and cure of the UV coating process at Total Door.

Total Door Color Match Capabilities

Another important feature of the Total Door UV system design and implementation is that the UV coating technology provides on-site color matching capabilities.

Conclusion

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Allied PhotoChemical Inc., Kimball, MI
Michael Kelly is president and chief executive officer of Allied PhotoChemical, Kimball, MI. He can be reached at 810/364.6910 or mkelly@alliedphotochemical.com.

Kevin H. Joesel is director of the Industrial Coatings Market segment for Fusion UV Systems, Inc., headquartered in Gaithersburg, MD, a manufacturer of industrial UV systems. Joesel can be reached at 248.486.7066 or KJoesel@fusionuv.com.

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • CEO of Total Door to Give Keynote Speech at RadTech Conference

    See More
  • UV Coatings Technology Delivers Best Economic Value Statement

    See More
  • What’s Next for the Coatings Industry When it Comes to Sustainability?

    See More

Related Products

See More Products
  • organic coatings.jpg

    Organic Coatings: Science and Technology, 4th Edition

  • Wood Coatings

  • 9780323355957.jpg

    Adhesives Technology Handbook, 3rd Edition

See More Products

Related Directories

  • Keyland Polymer UV Powder LLC

    Keyland Polymer develops, formulates, manufactures and sells UV cured powder coatings for wood, plastic, metal, composites, and other substrates. Keyland Polymer has a complete resin synthesis lab with global reach and distribution capabilities for the development, formulation, testing, and manufacturing of UV/EB curable solid resins.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing