Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Hyperbranched Polymers for Hardcoat With Superior Performance

February 8, 2006
Click for larger image


Combining environmental and productivity benefits, UV/EB technology is attractive for hardcoat applications, as high abrasion resistance can be achieved. Wood coatings, CD/DVD, LCD displays for mobile phones, touch-panel displays, and polycarbonate headlamp applications are examples where Radcure technology is well established. However, new applications like flexible displays, the new generation of electronic storage devices (HD-DVD, Blu-Ray) or in-mould decorations also mean new requirements like improved dimensional stability, higher flexibility, lower viscosity and better adhesion.

In this paper, we present a new precursor for the preparation of acrylic esters based on hyperbranched aliphatic polymer polyols. The unique molecular structure of the hyperbranched polymers provides high functionality at low viscosity and allows further improvements in all above-mentioned properties, compared to state-of-the-art high-functionality acrylates typically used in hardcoats like di-pentaerythritol hexaacrylate. A unique combination of properties such as high hardness, scratch resistance and flexible hardcoats with low viscosity and low shrinkage can be achieved.

Click for larger image

Introduction

Since the first synthesis of a dendritic polymer in the late 70´s, there has been growing interest for this new family of polymers because of their unique and specific properties compared to their conventional linear and branched homologues (see Hult1 and Fréchet2 for a review). They are obtained by reacting a poly-functional core with ABx monomers, typically AB2 monomers, yielding a "tree-like" amorphous structure (dendron means tree in ancient Greek). The obtained macromolecule is thus characterized by an exponential growth in both molecular weight and end group functionality.

Dendritic polymers (Figure 1) have traditionally been classified into two categories: dendrimers and hyperbranched polymers. A dendrimer is characterized by a perfectly symmetrical globular shape that results from a step-wise controlled process giving a monodispersed molecular weight distribution. The second category, the hyperbranched polymers, are attractive because they resemble dendrimers (their difference lies in their polydispersity and the less perfect globular shape) but they can be produced more easily on a larger scale and at a reasonable cost, thus making them commercially available in large quantities today.

Click for larger image
Unlike conventional polymers, the high number of end groups and their nature participate actively in the physical properties (solubility, glass transition temperature and viscosity) in combination with the backbone structure. This characteristic is exceptional since it leads to the possibility of designing the macromolecule with the combination of many different end groups, thus defining the type of reactive chemistry, properties and applications. The lack of entanglement results in a Newtonian behaviour with lower viscosity than the linear homologues (i.e., same nature and molecular weight). The solution viscosity is furthermore only slightly dependent on the molecular weight.3

The applications are numerous, and some important polymer fields can be mentioned, such as:

  • polymer additives (i.e., processing aids, compatibilizers for thermoplastics, toughener agents for thermosets4 and polyurethane foams5); and
  • polymer building blocks for coatings6,7,8 (i.e., high solid alkyds, powder coatings and radiation-curable coatings).


Click for larger image

Dendritic Polymers for Radiation-Curing Technology

Dendritic Polymers for Radiation-Curing Technology Radiation-curable technology is an ideal application to explore all the potential of such a macromolecule used as a building block. The combination of its characteristics makes the dendritic polymer a unique and promising candidate to today's stringent coatings quality requirements. The fundamental specific properties of dendritic polymers and their potential impact on coating performances are summarized in Figure 2.

Furthermore, the versatility of the technology (the type of core, the nature of the backbone, the number of generations and the shell structure) provides a wide range of different properties (viscosity, reactivity and flexibility/hardness). An appropriate design can lead to specific desired properties for any particular application.

A low-viscosity dendritic polymer has already been developed especially for radiation-curing applications10 exhibiting the mentioned performances like low viscosity at high molecular weight, high wear resistance and low extractables.

Click for larger image

Properties of the Hyperbranched Polyol

The hyperbranched polymer used to prepare the acrylic ester used in this study is a new, clear, low-viscosity hydroxyl-functional aliphatic hyperbranched polyester/ether blend called Boltorn® P500 having characteristics given in Table 1.

The characteristics of the acrylated hyperbranched polyol synthesized according to a conventional esterification process with acrylic acid are presented in Table 2. A simple comparison of viscosity as a function of molecular weight for five types of conventional oligomers used in radiation curing is given in Figure 3.

Click for larger image

Coating Characterization

Basic Comparison

The new dendritic acrylate was compared with two other high-functionality acrylates, di-pentaerythritol penta/hexaacrylate (DPHA, acrylic ester of di-pentaerythritol, polyol obtained from Perstorp Specialty Chemicals AB, Sweden) and an ethoxylated pentaerythritol tetraacrylate (acrylic ester of Polyol R4631, a tetrafunctional polyether polyol from Perstorp Specialty Chemicals AB, Sweden). All tests were done with 3% Irgacure 500 obtained from CIBA, Switzerland. The UV-curing unit was a Fusion F600 equipped with one H bulb.

As noted in Table 3, the new dendritic acrylate exhibited the following characteristics:

  • a significantly lower viscosity than DPHA;
  • as good surface cure as DPHA and better than Polyol R4631 acrylate;
  • as good flexibility as Polyol R4631 acrylate;
  • almost as good hardness as DPHA; and
  • almost as good water and ethanol resistance as DPHA.


Click for larger image
Scrub Scratch Resistance

Scratch resistance was evaluated by Scotch-Brite (green) rubs (constant weight of 500 g) and by measuring gloss retention (20º and 85º) as a function of cycles (50, 100, 150 and 200 rubs) and a UV dose of 500 mJ/cm2, 2 pass at 12 m/min for 40 µm thick films on black panels). The results are reported in Figure 4.

The new dendritic acrylate and DPHA demonstrated a very high scratch resistance as seen by gloss retention. It was significantly better than the tetrafunctional Polyol R4631 acrylate and similar to the DPHA.

Click for larger image
Hardcoats on Polycarbonate (PC)

The influence of the substrate is important for pencil hardness, especially at low film thickness (as compared to hard substrates like glass). A basic comparison was performed on polycarbonate sheet (Lexan 8010C, 250 µm, from GE) for the pure acrylates cured with 3% Irgacure 500 under a 160 W/cm H bulb in air. The coatings were conditioned at 25 °C and 50% RH for 24 hours before testing.

The new dendritic acrylate yielded similar pencil hardness as DPHA at high film thickness as shown in Table 4. The new dendritic acrylate exhibited significantly better adhesion than DPHA on PC (Table 5) as well as better flexibility as shown in Table 6.

Click for larger image
Topcoat Scratch Resistance and Accelerating Weathering

The scratch resistance and accelerating weathering performance of a UV topcoat based on Boltorn P500 acrylate was compared with a 2K isocyanate coating based on acrylic polyol and HDI trimer. All coatings were formulated with UV absorber and hindered amine light stabilizers (HALS) and a proper choice of photoinitiators was used for the UV formulation.

The UV topcoat formulations based on Boltorn P500 acrylate were cured with a total UV dose of 2000 mJ/cm2 under an H bulb from Fusion (F600). The UV coating exhibited largely superior scratch resistance (pencil hardness and scrub test) compared to the 2K isocyanate coating as shown by the results given in Table 7 and Figure 5.

The accelerated weathering performances of the topcoats were investigated on blue metallic waterborne basecoats. The panels were subjected to the alternate effects of condensation (4 hours at 50 °C) and the damaging effects of sunlight simulated by the fluorescent UVA lamps (4 hours at 60 °C).

Gloss (60°) and delta E were measured as a function of exposure time. The results (Figure 6) show that the Boltorn P500 formulation performs more or less as good as the reference 2K isocyanate based on HDI trimer and polyacrylic polyols with a gloss retention superior to 90% and a delta E inferior to 2 after 2000 hours of accelerated weathering exposure. Long-term exterior durability tests are currently running.

Click for larger image

Conclusion

The dendritic acrylate based on the new hyperbranched polyester/ether polyol blend Boltorn P500 is an excellent precursor for the preparation of hard, yet flexible acrylic esters providing the following benefits compared to other high-functionality acrylates:

  • a low-viscosity, high-functionality acrylate, much lower viscosity than DPHA, allowing easy formulating of low viscosity formulations with a high degree of latitude;

  • very good pencil hardness, almost as good as other high-functionality acrylates such as di-pentaerythritol penta/hexaacrylate (DPHA);

  • excellent scratch resistance, as good as DPHA and largely superior to a 2K isocyanate coating;

  • excellent water and ethanol resistance;

  • good flexibility, much better than DPHA;

  • very good adhesion to plastics, for example polycarbonate; and

  • good accelerating weathering performance.

Acknowledgement
The authors would like to thank Dogan Nazire from Akzo Nobel Car Refinishes, NL for supplying the primer and basecoat panels.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Paint and Coating Market Reports
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • pci0219-BASF-1076482774-900.jpg

    An Epoxy Curing Agent with Superior Carbamate Stability

    See More
  • BASF Expands Distribution Agreement With Superior Materials

    See More
  • [Hotel’s Contemporary Color-Changing Exterior Enhanced with Superior Coating System

    Hotel’s Contemporary Color-Changing Exterior Enhanced with Superior Coating System

    See More

Related Directories

  • Innospec Performance Chemicals

    Innospec is a global supplier of specialty chemicals for many different markets, including construction, emulsion polymerization, paint and coatings, polymers and waxes. Our innovative and responsible solutions cover a strong portfolio of additives and technically advanced solutions: rheology modifiers, anionic emulsifiers, wetting agents and dispersants.
  • Mallard Creek Polymers

    MCP provides a diverse line of acrylic, styrene-acrylic, and styrene-butadiene water-based emulsion polymers for the paints and coatings industry.
  • Mallard Creek Polymers

    MCP provides a diverse line of acrylic, styrene-acrylic, and styrene-butadiene water-based emulsion polymers for the paints and coatings industry.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing