Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Novel, Waterborne, Chlorine-Free Adhesion Promoter for TPO Substrates

By Ken-ichi Fujino, Kazuaki Minehata
November 1, 2007


Due to the high chemical stability, low price, excellent balance of physical properties, possible recycling, etc., the amount of polypropylene (PP) and thermoplastic olefin (TPO) consumed by automotive parts, household electrical appliances and the molded general goods businesses continues to increase. However, PP and TPO are plastics with low surface energy that make painting and adhesion problematic, hence chlorinated polyolefin (CPO) or chlorine-free modified polyolefin (CFPO) resins have found wide use as adhesion promoters.

In recent years, waterborne adhesion promoters applied to TPO substrates have been widely studied for use as both interior and exterior automobile coatings due to an increasing environmental awareness by industry. Furthermore, the automotive coatings industry desires waterborne coatings for TPO substrates that coalesce and adhere well at low baking temperatures, such as 80

Figure 1

Experimental

Polyolefin Starting MaterialsPolyolefin with different propylene content: Three different propylene-based polyolefins with relatively low crystallinity and Tm were used as the starting materials of WCFPOs. z-PO is a traditional polyolefin polymerized with a Ziegler-Natta catalyst and contains a smaller amount of propylene than the other polyolefins. m-PO is a metallocene polyolefin and has as low a Tm as z-PO, although the propylene content is much higher than that of the z-PO. m-PP is also polymerized with a metallocene catalyst, but without any ethylene and other a-olefin monomers. The crystallinity and the Tm of m-PP are low enough due to the low tacticity. The starting materials were chosen for each resulting WCFPO to have a similar molecular weight, Tm, and a minimum film formation temperature (MFT).

m-PP with different Tm: To further investigate the m-PP, three different WCFPOs were prepared with m-PPs having different Tm adjusted by their tacticities. The resulting WCFPOs were submitted to an exterior coating performance test.



Table 1

Preparation of WCFPO

Each polyolefin starting material was graft-modified with maleic anhydride and other acrylic monomers in the melt state. The content of maleic anhydride and acrylic monomers was approximately 2.0 and 1.5 wt% in the modified polyolefin, respectively. The modified polyolefin was emulsified with a nonionic surfactant and a neutralizer (ammonia) and then the solid content was adjusted to 30 wt%. Five WCFPO samples were prepared and their physical properties are shown in Table 1. The weight average molecular weights (Mw) and the molecular weight distributions (Mw/Mn) were measured with gel permeation chromatography [(GPC) Tosoh, GMHHR-H (S) HT, eluent: 1, 2, 4-trichlorobenzene, temperature: 145

Measurement of Tensile Strength

Tensile strength of the modified polyolefin was evaluated with the following condition. The modified polyolefin was compression-molded and cut to dumbbell-shaped specimens (#2 JIS) with the thickness of about 1 mm. Then the tensile strength was measured with a universal testing machine Tensilon RTC-1325A (A&D Co., Ltd.) at the rate of 200 mm/min, 23 

Figure 2

Peel Strength

Figure 2 shows the peel strength of WCFPOs onto three different polyolefin substrates. Each substrate coated with WCFPO was processed either at 80

Table 2

Exterior Coating Performance Test

The m-PP based WCFPO-3 showed very interesting properties in the tensile strength test and the peel strength test as compared with the z-PO based WCFPO-1 and the m-PO based WCFPO-2. It was interesting for the authors to see the availability of the m-PP based WCFPO in the field of automotive coatings. In this study three m-PP based WCFPOs with different Tm were prepared by adjusting the tacticity and the exterior coating performance test was conducted. The results are shown in Table 2.

The adhesion improved as the Tm of the WCFPO decreased, but on the other hand the gasoline resistance is better as the Tm of the WCFPO increased as long as the film formation was sufficient at this baking temperature. The film formation of WCFPO-5 was not sufficient at 80

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Ken-ichi Fujino | Nippon Paper Chemicals Co., Ltd, Iwakuni, Japan
Kazuaki Minehata | Nippon Paper Chemicals Co., Ltd, Iwakuni, Japan

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Paint and Coating Market Reports
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • Waterborne, Chlorine-Free Adhesion Promoter For TPO

    See More
  • Lead Image.png

    Waterborne Conductive Primer/Adhesion Promoter with Graphene Nanotubes

    See More
  • MD3 UV adhesion promoter for ACM panels.png

    UV Adhesion Promoter Enhances Ink Durability on Challenging Substrates

    See More

Related Products

See More Products
  • Adhesion, Surface Aspects & Coatings Defects (Virtual Course - 10/22/26)

  • laser tech.jpg

    Laser Technology: Applications in Adhesion and Related Areas

See More Products

Events

View AllSubmit An Event
  • October 30, 2025

    Novel Spherical Calcium Silicate Anti-Corrosion Pigment for Protective Coatings

    ON DEMAND: This presentation introduces a novel spherical calcium silicate as an effective anti-corrosion pigment for protective coatings. The modified spherical silica was synthesized using a unique patented manufacturing process, allowing to produce AC pigments with increased effectiveness for passivation, as well as easier and more even dispersion.
View AllSubmit An Event
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing