Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

The Use of Specialty Acrylate and Methacrylate Monomers in Emulsion Polymerization

January 18, 2006
The objective of this paper is to evaluate selected hydroxyl functional mono metha¬crylates, as well as reactive surfactants in emulsion polymerization (EP). Some of the selected hydroxyl functional monomers are extensively used as reactive diluents for radiation-curable adhesives and coatings. They are also used as capping agents in urethane methacrylate oligomers for the production of photopolymer printing plates and dry film resists.

The objective of this paper is to evaluate selected hydroxyl functional mono metha¬crylates, as well as reactive surfactants in emulsion polymerization (EP).

Some of the selected hydroxyl functional monomers are extensively used as reactive diluents for radiation-curable adhesives and coatings. They are also used as capping agents in urethane methacrylate oligomers for the production of photopolymer printing plates and dry film resists. In addition, they can be used in the production of acrylic polyols and urethane acrylate oligomers for use in photo imaging applications such as printed circuit boards. Other applications include the preparation of hydrogels, polyurethane dispersions, printing inks, water-reducible resins, etc. Now, the interest is to examine their incorporation characteristics, performance and benefits in emulsion polymerization.

Conventional (Non-Reactive) Surfactants

Emulsion polymerization technology has been discussed in a number of publications.1-4 The primary role of surfactants in EP is to lower the interfacial tension, which allows the emulsification of reactive vinyl monomers and the formation of stable colloidal dispersions of polymer particles. Conventional surfactants aid in the emulsification of monomers inside the micelles, stabilize the polymer particles during nucleation and growth, and promote the stability of the resulting latex.1-9 A fundamental property of surfactants is their ability to orient and adsorb at the interfaces. In latex systems, most of the surfactant is adsorbed at the interfaces between the particles and the water. This adsorption is a thermodynamic process favored by a decrease in the overall free energy of the system. The adsorbed layer of surfactant molecules is essential for the stabilization of latexes during polymerization and during post polymerization processes.

It is well known that the amount and chemical structure of the surfactant/s used in EP have a strong influence on conversion, particle size and distribution, viscosity, overall latex stability and cleanness. Surfactants also have an effect on final properties such as film formation, adhesion, wet ability, water resistance and foamability. A critical issue in the manufacture of commercial latexes is their stability during and after production.

As mentioned before, surfactants have an effect on overall latex stability. The appropriate selection of surfactants is an important consideration when designing a latex formulation. The most effective and widely used surfactants in EP are anionics and nonionics. Anionic surfactants prevent coagulation by electrostatic repulsions originated from the anionic charges adsorbed on the polymer particles and their associated double layers. Nonionic surfactants, especially polyethoxylates, prevent coagulation by spatial or steric stabilization.10-15,22 Some specialty surfactants, such as fatty alcohol ether sulfates, combine both electrostatic and steric stabilization in their molecules. The experimental section contains examples.

Reactive Surfactants

Reactive surfactants can be covalently bonded to the polymer. The most apparent advantage of bonding to the polymer is the minimization or elimination of surfactant migration to the interfaces during film formation, which may increase water resistance, adhesion, latex stability and decrease foaminess. An extensive number of references have been provided elsewhere.16-20

Reactive surfactants can be classified as surface-active initiators, i.e. surfactants with an initiating moiety (inisurfs); surfactants bearing a moiety capable of chain transfer (transurfs), or surfactants with a functional group capable of copolymerization (surfmers). This discussion is about surfmers, or reactive surfactants having at least one vinyl bond capable of reacting via free radical polymerization, and a surface-active moiety in their molecules. A caveat related to surfmers is the difference in surface activity shown during incorporation in EP. Some surfmers can be used as the sole reactive emulsifier to carry out a polymerization to full conversion. Others need to be combined with a co-surfactant to produce a stable polymer.

The next section summarizes results obtained using two reactive surfactants: TREM™ LF-40, a sodium dodecylallyl sulfosuccinate and Bisomer® SEM, an ammonium sulfatoethyl methacrylate (sulfated HEMA). TREM LF-40 has been the topic of numerous studies at Lehigh University.16-20 It can be used as the sole emulsifier to carry out a polymerization to full conversion. Bisomer SEM was found effective replacing up to 80% of a conventional anionic surfactant. Therefore, when using Bisomer SEM, at least 20% of a co-surfactant, typically anionic in character, would be needed to produce stable latexes. Combinations of Bisomer SEM and Disponil® FES 32, a fatty alcohol ether sulfate of composition C12-14, [4-ethylene oxide moles] Na sulfate, are very effective in the preparation of nanolatexes. It has also been observed that the incorporation of Bisomer SEM increased the overall stability and the water resistance of latexes. For example, the experimental session illustrates that latexes made with a combination of Bisomer SEM and anionic surfactants had better stability and water resistance than latexes made with a conventional anionic surfactant as the sole emulsifier.

(Click image for larger view)

Hydroxyl Functional Monomers

The hydroxyl functional monomers studied are adducts of polyethylene glycol or polypropylene glycol with hydroxyl monomers. They consist of a range of hydroxyl functional monomethacrylates with different molecular weights, different hydrophilic and hydrophobic characteristics, and different reactivity. The adducts evaluated have low glass transition temperatures (Tg), making them ideal for internal plasticization of polymers. The pendant hydroxyl functionality is suitable for further chemical modifications such as chain extension, grafting and crosslinking.

(Click image for larger view)

Experimental

Performance of Reactive Surfactants: Pressure Sensitive Adhesive Formulation

Table 1 summarizes the performance of reactive surfactants TREM LF-40 and Bisomer SEM in a vinyl acrylic pressure sensitive (PSA) formulation. The results of incorporating these two reactive surfactants at 0.5% based on total monomer content is compared to the control polymerization run made without either of them. The chemical structures of the reactive surfactants are shown in Figure 1.

The incorporation of either reactive surfactant in the formulation did not have a noticeable effect on most of the physical properties of the latexes. The coagulum content, the viscosity and the particle size and distribution, as well as the overall stability were similar to those given by the control polymerization run. However, the water resistance was remarkably increased in latexes containing either reactive surfactant.

The water sensitivity was evaluated on latexes coated on untreated aluminum panels. Drops of water were placed on the surface of the coatings. The film appearance was recorded at several intervals during eight hours. A significant improvement in water resistance was observed in the coatings made with TREM LF-40 and Bisomer SEM.

The latexes were also coated on polypropylene film and laminated to the same. The peel adhesion was determined using an automated Thwing Albert peel tester.

The laminates made with the latexes containing reactive surfactants showed improved peel adhesion over the control. However, the improvement in water resistance was substantially higher than the improvement in peel adhesion.

(Click image for larger view)

Performance of Hydroxyl Functional Adducts in Architectural Coatings

Sabatier and Glaze21 reported the advantages of polypropylene glycol monomethacrylate, Bisomer PPM6E, as an internal plasticizing co-monomer in the preparation of low-VOC vinyl acrylics for paint binders. PPM6E was found to be effective as a partial or total replacement of low-Tg monomers such as butyl acrylate (BA) and vinyl versatate (VV10). The report illustrates the plasticizing efficiency of PPM6. It was shown that 8% of PPM6E was equivalent to 13% BA or 18% VV10. The vinyl acrylic binders were formulated with protective colloid (HEC) and several nonionic surfactants and stabilizers.

The structures of the mono¬methacrylate adducts used in this study are shown in Figure 2. These are suitable alternatives to HEA and HPA, as they are non-toxic, easy-to-handle, low-viscosity clear liquids, and polymeric by EINECS classification.

Due to its propylene glycol segment, Bisomer PPM5S is the most hydrophobic of the monomers shown; its hydroxyl functional group is secondary. Bisomer PEM63P and PPM63E combine short ethylene glycol and propylene glycol blocks. Different combinations of glycol blocks provide different water/monomer solubility and reactivity. In addition, either PO/EO or EO/PO blocks present alternative pendant primary and secondary hydroxyl terminal functionalities. The primary hydroxyl is more reactive and may offer potential benefits to further crosslinking for scratch-resistant coatings.

This experimental section discusses the effect of replacing low-Tg monomer butyl acrylate with the described monomethacrylate adducts. These adducts have a plasticizing efficiency equivalent to a glass transition temperature of -70 °C (21), which make them very suitable to replace commercial internal plasticizing monomers such as 2-EHA, DOM and IOA. A significant benefit of using the adducts as internal plasticizing monomers could be the preparation of low-VOC acrylics and vinyl acrylics for architectural binders.

The vinyl acrylic latexes evaluated in this study were made without protective colloids. A current trend in the production of binders for architectural coatings is the ever-smaller particle sizes to improve film integrity, water and humidity resistance, as well as alkali resistance. The appropriate combination of anionic surfactant Disponil FES 77, a fatty alcohol ether sulfate of composition C12-14 with [30-ethylene oxide moles] Na sulfate, and nonionic surfactant Disponil AFX 4060, a modified fatty alcohol ethoxylate of composition C12-14 with [40-ethylene oxide moles], gave the desired particle size and distribution and overall stability. The long polyglycol ether hydrophilic moiety in these surfactants provided sufficient steric stabilization to produce stable latexes. The acrylic terpolymers were made using a very effective anionic surfactant, Disponil FES 32, which gives an excellent balance of desired particle size and overall latex stability.

In this study, several Bisomer adducts were evaluated in two model formulations, a vinyl terpolymer and an acrylic terpolymer. The control vinyl acrylic had a composition consisting of 76% vinyl acetate, 23% butyl acrylate and 1.5 % methacrylic acid. While the control acrylic had a composition of 51.5% methyl methacrylate, 47% butyl acrylate and 1.5% methacrylic acid. As mentioned before, a significant benefit of using the adducts as internal plasticizing monomers could be the preparation of low-VOC acrylics and vinyl acrylics for architectural binders.

To evaluate this potential benefit, some of the latexes were formulated into paints with and without coalescing agents in the formulation. Table 2 shows the effect of incorporating the three previously described Bisomer adducts in the model vinyl acrylic terpolymer. The concentration of the adducts replacing BA in the control latex is shown in the table. The latexes containing the adducts showed a decrease in the MFFT of approximately 8-7 °C.

All of the latexes were formulated into a flat paint formulation with and without coalescing agent. Preliminary results indicated that it is feasible to prepare good film-forming paints without coalescing agent.

Table 3 shows the effect of incorporating two previously described Bisomer adducts in a model acrylic terpolymer. It is important to point out that Disponil FES 32, a fatty alcohol ether sulfate of composition C12-14 [4-ethylene oxide moles] Na sulfate, is an effective surfactant to produce fine-particle-size latexes. However, the latex formulated with 1% surfactant concentration did not pass the freeze-thaw stability test. Typically, the freeze-thaw stability can be restored or obtained by post adding 1% of a steric stabilizer such as Disponil AFX 4060 or Disponil AFX 5060. Disponil AFX 4060 is a modified fatty alcohol ethoxylate of composition C12-14 [40-ethylene oxide moles]. Disponil AFX 5060 is a modified fatty alcohol ethoxylate of composition C12-14 [50-ethylene oxide moles].22 However, for some sensitive applications, the addition of surfactants after polymerization often produces undesirable water sensitivity, and therefore the evaluation of selected adducts may be appropriate.

As Table 3 shows, the latexes made by replacing 5% of BA with Bisomer adducts PEM63P and PPM5 passed the freeze-thaw test. Freeze-thaw is a very desirable physical property; thus, these results may be useful in designing formulations with improved F/T stability.

(Click image for larger view)

Summary

The reactive surfactants TREM LF 40 and Bisomer SEM were very effective in improving the water resistance of a PSA formulation. Plasticizing Bisomer adducts PPM5S, PEM63P and PPM63E were evaluated in a vinyl acrylic formulation for architectural coatings replacing 10% BA. The resulting latexes showed comparable overall stabilization to the control polymerization and decrease in MFFT of approximately 8-7 °C. Preliminary results indicate that it is feasible to prepare low-VOC and good film-forming paints without coalescing agent. Paints containing adduct PEM63P had improved wet ability as measured by the fewer defects observed in the films.

In addition, the replacement of BA with Bisomer adducts PEM63P and PPM5 produced acrylic latexes with improved freeze-thaw stability. A significant benefit of using the adducts as internal plasticizing monomers could be the preparation of low-VOC acrylics and vinyl acrylics for architectural binders, the improvement of overall stability and in some instances the improvement in substrate compatibility and wet ability.

References

  1. Harkins, W.D. J.Am. Chem Soc. 1947, 69, 1428.
  2. W.V. Smith, W.V.; Edwards, R.H. J. Chem. Phys. 1948, 16, 592.
  3. Smith, W.V. J. Am. Chem. Soc. 1949, 70, 3695, 1948, ibid. 71, 4077, 1949.
  4. Blackley, D.C. Emulsion Polymerization. Applied; Sci. Publishers Ltd., 1975.
  5. Fernandez, A.M.; Evans, E.; Held, U.; Feustel, D.; Natale, M.; Tuttle, B.; Klima, R. International Waterborne Symposium, 1999.
  6. Piirma, I.,et.al. J. Polym. Chem. 1982, 20, 489.
  7. Piirma, I., et.al. Polym. Bulletin 1984, 11, 497.
  8. Medvedev, S.S., et.al. J. Macromol.Sci. Chem. 1973, 7, 715.
  9. Fernandez, A.M.; Saint Victor, M.E., et al. International Waterborne Symposium, February 2004.
  10. Okamura, S. et. al. J. Polym. Sci. 1962, 58, 221.
    11 Fernandez, A.M.; Saint Victor, M.E., et al. Federation of Societies for Coatings Technology, October, 2004.
  11. Verwey, E.J.W.; Overbeek, J.G. Elsevier, 1948
  12. Naper, D.H. Sci. Prog. Oxford, 1967, 55.
  13. Napper, D.H. Trans. Faraday Soc. 1969, 64.
  14. Napper, D.H. J. Colloid. Interface Sci. 1970. 32.
  15. Sudol, E.D,; El-Aasser, M.S. Advances in emulsion polymerization and latex technology-EPI, Lehigh University.
  16. Urquiola, M.B.; Dimonie, V.L.; Sudol, E.D.; El-Aasser, M.S. J.Polym. Sci., Part A: Polym. Chem. 1992, 30, (2619 and 2631).
  17. Urquiola, M.B.; Dimonie, V.L.; Sudol, E.D.; El-Aasser, M.S. J.Polym. Sci., Part A: Polym. Chem. 1993, 31,1403.
  18. Wan, X. "Emulsion polymerization of styrene using a reactive surfactant".Ph. D. dissertation thesis, EPI, Lehigh University, 2000.
  19. Wan X.; Sudol, E.D.; El-Aasser, M.S. ACS Symposium Series, 2002.
  20. Sabatier, L.; Glaze, A.P. JOCCA, 1993.
  21. Fernandez, A.M. ; Saint Victor, M.E., et al., Federation of Societies for Coatings Technology, October, 2004.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Paint and Coating Market Reports
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • The Use Of Specialty Acrylic Esters In Cure-In-Place Coating Technology

    See More
  • Rohm and Haas Declares Force Majeure on Acrylate, Methacrylate and Specialty Monomers

    See More
  • Self Crosslinking Polymeric Dispersants Used in Emulsion Polymerization

    See More

Related Products

See More Products
  • Principles and Applications of Emulsion Polymerization

  • durability.jpg

    Increasing the Durability of Paint and Varnish Coatings in Building Products and Construction 1st Edition

  • hetrophase.jpg

    Heterophase Polymerization: Basic Concepts and Principles

See More Products

Related Directories

  • Miwon North America Inc.

    Miwon Specialty Chemical offers a wide range of high-performance products for the paint and coatings industry. The MIRAMER™ range includes acrylate and methacrylate monomers, specialty oligomers, benzoin, sucrose benzoate (SB), and PUD acrylates. With 13 global locations, we deliver innovative solutions and outstanding support to meet industry needs.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing