Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Industry Update: Molybdate Corrosion Inhibitors

February 26, 2001
In response to the ongoing elimination of chromate- and lead-based pigments and the need to identify effective replacements, molybdate corrosion inhibitors are finding increased application in the coatings industry. The key advantages associated with the use of these pigments as environmentally friendly corrosion inhibitors include the following.

  • Molybdate corrosion inhibitors represent field-proven technology, demonstrated in numerous outdoor exposure studies and supported by over 30 years of commercial use in the industry.

  • Molybdate corrosion inhibitors are effective in both conventional salt-spray tests and the newer cyclic salt-spray/UV exposure tests (e.g., ASTM D 5894) being used by the industry.

  • Molybdate corrosion inhibitors are available in a range of pigment chemistries, thus allowing for more effective application in specific systems.

  • Molybdate corrosion inhibitors are also now available in easy-dispersing, micronized grades, offering a finer, more narrow particle size distribution for optimized performance in thin-film applications (e.g., under 1 mil).

    This article presents a review and update on molybdate corrosion inhibitor technology, with particular emphasis on recent testing of calcium zinc phospho-molybdate and easy dispersing, micronized molybdate inhibitors.

    Table 1 / Chemical and Physical Properties of Commercially Available Molybdate (Moly-White®) Corrosion Inhibitors

    Background

    Molybdate corrosion inhibitors have been used in the coatings industry since the early 1970s. These pigmentary materials are produced using a patented process whereby active molybdate compounds (e.g., zinc molybdate or calcium zinc molybdate) are deposited onto relatively inert carrier pigments (e.g., zinc oxide or calcium carbonate) for optimized use of available molybdenum and reduced raw material costs.

    The protective action of molybdate pigments is based on the slight solubility characteristics of zinc and calcium molybdate compounds coupled with the well-recognized corrosion inhibiting action of molybdate ions in aqueous solution. When a coating film containing molybdate corrosion inhibitors is immersed or exposed to water, small quantities of molybdate ions will be released into the coating film. These molybdate ions will then interact with the metallic substrate to promote the formation of an adherent oxide layer, which prevents corrosion of the underlying substrate. This process is described as passivation.

    Various product modifications in terms of chemistry, molybdate content and core pigmentation, have resulted in the availability of a range of commercially available molybdate corrosion inhibitors.

    A series of phospho-molybdate pigments has also been introduced. These products were developed based on a synergistic action between phosphate and molybdate compounds in corrosion inhibition processes.

    This range of molybdate pigments (see Table 1) has allowed for more optimized applications in specific types of coatings. Molybdate corrosion inhibitors are today used commercially by major industrial coating manufacturers in the United States, Europe, South America and Asia.

    Table 2 / Styrene Acrylic Latex Primer with Calcium Zinc Phospho-Molybdate

    Calcium Zinc Phospho-Molybdate

    The performance of the newer phospho-molybdate pigments was recently studied in the testing of a series of waterborne and high-solids coating formulations. In particular, calcium zinc phospho-molybdate was found to be a highly cost-effective and versatile corrosion inhibitor based on testing in the following systems. • Styrene acrylic latex primer • 2K waterborne epoxy primer • Water-reducible alkyd primer • 2K high-solids epoxy primer

    Table 3 / Waterborne 2K Epoxy Primer with Calcium Zinc Phospho-Molybdate (4:1 mix ratio)
    In each of these studies, a model formulation (provided by the resin supplier) was used to evaluate the performance of calcium zinc phospho-molybdate vs. other corrosion inhibitors.

    Figure 4 / 2K High-Solids Epoxy Primers after Accelerated Testing (substrate: hot rolled blast steel, dft: 3.0 mils, inhibitor loadings: 1.0 lbs/gal)
    The formulas for the calcium zinc phospho-molybdate based coating systems are shown in Tables 2–5. In all cases, corrosion inhibitors were tested and compared by substituting different inhibitors at an equal weight addition level in the formulas.

    Table 5 / 2K High-Solids Epoxy Primer with Calcium Zinc Phospho-Molybdate (4:1 mix ratio)
    Small adjustments in extender levels, to maintain equal PVC and volume-solids, were the only other differences between the formulations.

    Figure 1 / Styrene Acrylic Latex Primers after Accelerated Testing (substrate: cold rolled mild steel, dft: 2.2 mils, inhibitor loadings: 0.5 lbs/gal)
    Corrosion tests based on salt-spray (ASTM B 117) and cyclic salt-spray/UV exposure (ASTM D 5894) were then conducted to determine corrosion inhibitor effectiveness.

    Figure 2 / 2K Waterborne Epoxy Primers after Accelerated Testing (substrate: blast hot rolled steel, dft: 3.5 mils, inhibitor loadings: 0.5 lbs/gal)
    Representative results are presented in Figures 1–4, which show the appearance of test panels at completion of the corrosion tests.

    Figure 3 / Water-Reducible Alkyd Primers after Accelerated Testing (substrate: cold rolled mild steel, dft: 1.2 mils, inhibitor loadings: 1.0 lbs/gal)
    Market pricing information is included in the figures so that some appreciation of cost-effectiveness can be gained.

    Figure 4 / 2K High-Solids Epoxy Primers after Accelerated Testing (substrate: hot rolled blast steel, dft: 3.0 mils, inhibitor loadings: 1.0 lbs/gal)
    Calcium zinc phospho-molybdate clearly provides excellent cost-effective performance based upon these results.

    Figure 5 / Polyester Coil Coatings after 1000 hr Salt-Spray Test - Duplicate Panels (substrate: phosphated cold rolled mild steel, dft: 0.6 mils, inhibitor loadings: 0.67 lbs/gal)

    Micronized Molybdate Corrosion Inhibitors

    Molybdate corrosion inhibitors are now available in standard and easy-dispersing, micronized forms. The micronized grades offer a finer, narrower, particle size distribution allowing for improved ease of dispersion, increased surface activity and optimized performance in thin-film systems (under 1 mil dft).

    A recent study was conducted in a thin-film solventborne polyester coil coating formulation to compare the micronized vs. the standard molybdate pigment materials. Here, calcium zinc molybdate and zinc molybdate, in standard and micronized forms, were incorporated in a polyester coil coating formulation (provided by the resin supplier). Also tested were strontium chromate and a number of other inhibitors recommended by suppliers for thin-film polyester coil coatings.

    The coil coating formulation based on micronized zinc molybdate is shown in Table 6. In all cases, corrosion inhibitors were substituted and tested at an equal weight addition level. Small adjustments in titanium dioxide levels were made to maintain constant PVC and volume solids.

    Table 6 / Polyester Coil Coating with Micronized Zinc Molybdate
    Figure 5 shows the results of salt-spray testing, which is the most crucial corrosion test used by the coil coatings industry. The micronized molybdate pigments allow for performance characteristics comparable to strontium chromate, a corrosion inhibitor still widely used in coil coatings and aerospace primers despite serious toxicity concerns.

    Conclusion

    The demonstrated performance capabilities of molybdate corrosion inhibitors, particularly calcium zinc phospho-molybdate and newly available micronized pigment grades, should allow for the continued growth of these important functional pigments.

    For more information, contact Moly-White Pigments Group, 601 Canal Road, Cleveland, OH 44113; phone 216/566.1294; fax 216/566.3837; e-mail chsimpson@sherwin.com; visit www.moly-white.com.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • Hexigone Joins Forces with MCassab to Supply Sustainable Corrosion Inhibitors in Brazil.png

    Hexigone Joins Forces with MCassab to Supply Sustainable Corrosion Inhibitors in Brazil

    See More
  • New "Eco-Friendly" Universal Corrosion Inhibitors

    See More
  • Novel Corrosion Inhibitors

    See More

Related Products

See More Products
  • corrosion of linings.jpg

    Corrosion of Linings & Coatings: Cathodic and Inhibitor Protection and Corrosion Monitoring

  • intelligent.jpg

    Intelligent Coatings for Corrosion Control 1st Edition

  • corrosion.jpg

    Corrosion Control Through Organic Coatings 2nd Edition

See More Products
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing