Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Metallic Pigments for Powder Coatings

January 1, 2003


Figure 1 World Powder Coatings Market
Metallic finishes have a luster and brilliance that sets them apart from finishes produced by conventional pigments. For many applications, a metallic effect is highly desirable and can be achieved by adding aluminum, gold bronze or pearlescent pigments. While it is relatively easy to incorporate such pigments into liquid systems, the situation is much more difficult for powder coatings. Various problems associated with the manufacture of metallic powder coatings and some solutions will be discussed.

The powder coatings market has grown considerably over the last 20 years. The current market is reported to be in excess of 1.76 billion pounds. Figure 1 shows that Europe still has the lion's share with about 45%, while the North American and Asian markets continue to grow. Although metallic coatings represent a small percentage of this total, they play a significant part in providing enhanced color opportunities in the marketplace.

Benda-Lutz has been manufacturing metallic pigments, including aluminum, gold bronze and zinc products, since 1910. The company is into its third decade of providing a global bonding capability. Benda-Lutz currently sells metallic pigments into applications including printing inks and coatings. The typical markets for metallic powder coatings include automotive components, architectural aluminum, office furniture, and lawn and garden applications. One reason that powder coating has proved so popular over the last 10 years is its lack of affect on the environment. Compared with liquid paint, it has a nearly perfect environmental profile with virtually zero VOCs, and no paint sludge residue, effluent disposal or noxious odors. The fact that powder coating can be reclaimed thus reducing the waste has also been significant in making powder coatings a viable alternative to existing technologies. However, collecting and re-using the overspray has caused specific problems with regard to metallic finishes.

Figure 2 Blitz Bonding

Effect Pigments

The most popular effect pigment is aluminum. Aluminum is available in both leafing and non-leafing grades, and in a range of particle sizes that enables the production of a variety of shades including chrome and sparkle effects. In addition, coatings with these pigments convey various properties to the final formulation. Other metallic pigments include a range of gold bronze pigments available as rich gold, rich pale and pale gold. For exterior coatings, stainless steel has proved very popular, although it lacks the luster of aluminum. In addition, a range of non-metallic pearlescent pigments are suitable for both interior and exterior applications. There are several techniques available for the manufacture of metallic powder coatings, including the following methods of incorporation.

Figure 3 Cyclone Test

Extrusion/Grinding

Extrusion/grinding involves premixing the metallic pigment with all the other ingredients of the formulation followed by extrusion using a single or twin-screw compounder. The extrudate is then milled to a controlled particle size and sieved. The main problem is that the shear forces destroy the metal particles and make it impossible to achieve the desired optical effect. Instead of high luster coatings, the process results in dull, gray coatings. Hammer finishes are usually produced by this technique.

Dry Blending

The process of dry blending metallic pigments into conventional powder coatings can produce satisfactory results in laboratory tests. However, in application plants where powder recovery is used, it is impossible to produce acceptable results without large color differences. In addition, varying phenomena can result including poor charging characteristics and pigment agglomerations particularly on the tips of the guns.

Standard Bonding

This represents the method we originally used, and is currently in use by some companies today. It offers an improvement over dry blending in that it provides improved application characteristics.

Blitz(tm) Bonding

In 1980, we introduced a technique for adding effect pigments to powder coatings. The process involves adhering the effect pigments to the powder coating particles to prevent separation during application and recycling. (Figure 2)

Following research during the 1980s and early '90s, a new continuous multi-stage process for bonding was introduced. The main advantage with the Blitz Bonding process is the degree of control over the entire operation. Batch size becomes less of an issue and there are significantly improved application characteristics. This process was successfully introduced into the United States during 1996. To develop the process, it was first necessary to have a viable method to determine that a product was correctly bonded. Several techniques have been developed to check for bonding quality, including photo microscopy, various charging techniques, and the cyclone test (see Figure 3).

Testing was carried out to quantify and compare the color difference effect caused by both dry blending and Blitz Bonding. Although it is difficult to obtain a single value for the color measurement, which is proportional to the pigment content, it was decided to use the lightness factor at five angles. The lightness curve of the base material is defined as 0% and the virgin metallic powder as 100%. Material was passed through the cyclone and L- values taken for each run at the five angles. After three runs the dry blended powder shows an effect loss of 50% (see Figure 4).

A similar exercise was carried out on the bonded sample and in this case even after three runs the lightness factor remains at 95% (see Figure 5).

All powder chemistries have been successfully Blitz bonded including hybrids, TGIC, Primid, and GMA acrylics.

Conclusion

Bonding effect pigments to powder coatings using the Blitz Bonding process offers the formulator and final end user significant advantages. These include the ability to take aluminum out of the plant and hence reduce the risks associated with handling aluminum. Above all, it allows the applicator to apply a consistent product with a constant metallic effect. These culminate in the powder manufacturer and end user achieving cost savings.

For more information on pigments, contact Benda-Lutz, Corp., 10500 Toebben Dr., Independence, KY 41051; phone 859/746.0392; fax 859/525.3012; e-mail office@benda-lutz.net; or visit www.benda-lutz.com.

Links

  • Benda-Lutz, Corp.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Paint and Coating Market Reports
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • pci0422-Shepherd-609811204-1170.jpg

    Problem-Solving Pigments for Powder Coatings: Durable, Functional and Colorful

    See More
  • ask joe powder pci

    Metallic Pigments in Powder Coatings

    See More
  • PCI Announces Plans for Powder Coatings Seminar

    See More

Related Products

See More Products
  • marketsandmarketslogo.jpg

    Metallic Powder Coatings Market by Process Type (Bonding, Blending, Extrusion)...

  • Kevin-Biller-PC-BOOK.jpg

    Powder Coatings - Foundation for the Novice Formulator (ebook)

  • Powder Coatings Processing (Virtual Course - 6/25/26)

See More Products

Related Directories

  • Schlenk Metallic Pigments

    SCHLENK supplies state-of-the-art metallic pigments, including solvent and waterborne aluminum and gold bronze pigments for all coatings and paint applications. In addition, we supply unique special effects like our Zenexo® ultra-thin colored aluminums that offer unmatched durable gold and orange effects. Our very broad Decomet® vacuum metallized pigment line allows formulators to achieve very smooth metal and chrome-like effects. SCHLENK products are available globally.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing