Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Mixed Mineral Thixotropes

By Dr. Klaus Dziwok
October 1, 2007
This paper concentrates on a new kind of thixotrope, which is based originally on organoclay chemistry, but spreads out the application areas to new grounds, showing unique properties – the mixed mineral thixotropes – or, in short, MMTs.

Figure 1


In the coatings industry, additive use and knowledge is always an important part of success. Little amounts can change the performance a lot. Among the widespread classes of additives the thickeners play an important role. Although they are just called “thickeners,” they are mainly thixotropes that give the coating its typical application and storage properties. The most widely used thixotropes are organoclays, fumed silicas and castor waxes. Among all applications, there are typical ones for each kind of thixotrope, defined by its inherent strength. This paper concentrates on a new kind of thixotrope, which is based originally on organoclay chemistry, but spreads out the application areas to new grounds, showing unique properties – the mixed mineral thixotropes – or, in short, MMTs.

Figure 2

MMTs - How They Work

The chemical bases of organoclays and MMTs are rather similar. Both are based on clays. The anionic clay surface is covered with cationic quaternary ammonium compounds to render it hydrophobic and compatible with organic coatings (Figure 1). The chemistry of thickening is expected to be rather similar. The hydrophobic clay platelets are separated by shear during dispersion. As only the faces of the platelets are covered by hydrophobic quaternary ammonium compounds, the edges of the platelets are still hydrophilic uncovered clay.

In an organic surrounding, the hydrophilic parts of different platelets interact with each other by hydrogen bonding. This gives a three-dimensional network and creates the thickened gel structure, also called the card-house effect (Figure 2). The gel has only a certain strength, which can be destroyed by shear force and builds up again at low shear conditions (Figure 3). This is always reversible. It gives the coating its thixotropic behaviour. Under no- or low-shear conditions like storage and application sag, the viscosity is high due to an intact gel. At brush or spray application the gel breaks down and does not give much viscosity. This is why organoclays are used as anti-sag, anti-sedimentation and anti-syneresis additives.

Figure 3

Up to this point organoclays and MMTs are rather similar. But what’s the difference then? It is the clay base. Typical organoclays are made out of uniform clay particles, e.g., bentonite or hectorite. MMTs are different. They are, by design, built out of several clays. They are built out of different clays with different-shaped particles. One may say this is just non-pure clay sources, but in fact this is done on purpose. Different-shaped clays are mined separately and are purified separately. Only at the step of rendering the surfaces hydrophobic are they packed together in one reaction vessel. The MMTs are patent protected.

Figure 4

The unique shape of these mixed minerals gives the MMTs its unique performance. Due to a mix of platelet-shaped, ribbon-shaped and pipe-shaped clays, the product particles cannot be stacked parallel and as dense as the uniformly platelet shaped conventional organoclays (Figure 4). The various particles are not as close to each other. They are not able to stick to each other strongly. Translated into application properties this means that the particles in MMTs can be separated from each other more easily than the particles in conventional organoclays. This gives quicker and easier dispersion, even easier than easy-dispersible conventional organoclays.

Figure 5

The microscopic structure can be seen in macro by exhibiting a lower bulk density compared to conventional organoclays. But compared to fumed silica, the density is still much higher (Figure 5). Even for MMTs that give a similar performance to fumed silica, it is easier to handle them due to their higher density. MMTs are less dusting and need less space in bags and warehouse.

Figure 6

Application

Even though MMTs are similar to conventional organoclays and similar in performance to fumed silica, they show several advantages. First is the possibility to create higher-concentrated pregels. It is possible to produce pregels at concentrations of 10 – 15% MMT that are still pourable and easy to handle. Also not much shear is needed to disperse MMTs. In some cases circulation pumps alone can do the job. For organoclays only about 6% pregels are possible and are already on the edge of pumpability. For fumed silicas it is even much less than that. The pregels of MMTs can be made not only in solvent, but also in monomers e.g., styrene. No activator is needed, and this is an advantage in high solids (Figure 6).

The application properties are also unique. The MMTs show a very pseudoplastic thickening. That means low high-shear viscosity during application of the coating, but high low-shear viscosity at rest, which gives superior anti-sag and storage stability.

Table 1

Examples

Case One
Typical systems where organoclays fail are high-solid systems. They give too much application viscosity or do not disperse at all. One system where the conventional organoclay failed is unfilled unsaturated polyester. Here the classical alternative was fumed silica. This formulation (Table 1) based on Gremopal unsaturated polyester resin is shown in a graphic (Figure 7).

Figure 7

The organoclay did not show the requested shear thinning viscosity. The fumed silica was better, but the MMT shows the optimum performance: low viscosity at application e.g., during spraying, but high low-shear viscosity. This gives the best anti-sag behaviour.

Table 2

Case Two
The second example is also an unsaturated polyester system based on Palatal P4-01 (Table 2). In this case organoclay was not even a choice, and fumed silica could be outperformed by MMT at optimized conditions. That means, when the MMT was added as a powder, the performance was quite similar to fumed silica. Anti-sag and flow curves were rather comparable, but MMTs show a unique advantage in this case. It is possible to make a 12% pourable pregel in the styrene monomer by low shear mixing. For fumed silica there was no way to make a pregel in the existing low amount of styrene in this formulation. When the MMT was prepared as a pregel, the performance was twice as good. MMT gives the same sag resistance and a similar flow curve at 0.5 % addition level compared to 1% fumed silica. The graphic in Figure 8 demonstrates this in detail. The storage stability of the MMT formulation was the best achieved compared to all competitive products, giving no syneresis and no sedimentation.

Figure 8

One of the reasons for the perfect behaviour of the MMTs can be demonstrated by doing a shear relaxation test. A coating containing a thixotrope is first mixed with high speed to destroy the three-dimensional structure of the thixotrope, which is responsible for the gelling of the coating. After that, the mixing speed is turned down to a low shear rate of 1 sec-1. How long it takes for the coating to recover its original viscosity is measured, which means how long it takes to rebuild the three-dimensional card-house structure again. In Figure 9 it can be demonstrated that the recovery in this system is quicker with MMT rather than with fumed silica. It is also obvious that the high shear viscosity of the MMT is lower, giving easier application and lower spray resistance.

Figure 9

In general MMTs don’t need an activator, but in some cases small amounts of enhancers help to improve the gel. Especially in unsaturated polyesters, enhancers are used to gel the fumed silicas. A test demonstrated an effect also on MMT. Only small amounts of approximately 10% enhancer based on MMT are sufficient to give improved gelling. Several enhancers have been tested. The typical activator for organoclays, propylene carbonate, is not the best. Preferred is Byk R605 or DGA (diglycolamine). In some cases just a little water is enough to give the best hydrogen bonding and the best gelling.

Table 3

Case Three
Another challenge for organoclays are epoxy resin systems, and here especially solvent-free epoxy coatings give few possibilities to optimize the dispersibility of conventional organoclays by low concentrated pregels. For dispersing MMTs only the epoxy resin itself may work. Compared to castor waxes and amide waxes, MMTs need no elevated temperature to disperse and, of course, show no seeding problems.

An example is shown in a 2-pack epoxy floor coating (Table 3), which contains quartz sand as a filler. Due to the high density of the quartz sand it settles out quickly and the mix is not storage stable without a thixotrope. MMT was compared with a conventional organoclay and a fumed silica. The picture in Figure 10 shows the storage test results. As expected, the organoclay is not suitable at all. Fumed silica and MMT work, with advantages for the MMT.

MMTs even work in solvent-free systems; it is recommended to use a 10-15% pregel in cases were solvents are used in the formulation in order to minimize the required amount of MMT. Also monomers, or the component with the lowest viscosity, might be used to prepare a pregel. In filled systems the advantage of a pregel is often not required as there is enough milling material available to fully disperse the MMT.



Figure 10

Case Four
Another system is shown where the conventional organoclay does not give the required performance and can be replaced by MMT. This is an unfilled 2-pack PU system. The conventional organoclays all failed in rendering the polyol part thixotropic. They just exhibit a Newtonian viscosity increase. This refers to insufficient dispersibility of the conventional organoclay. The only clay product working in the requested way is the MMT. It shows a pseudoplastic thickening. After adding the curing part, the sag was tested immediately. Also in this case, the MMT is still the product with the best sag resistance compared to all tested conventional organoclays (Figure 11).

Figure 11

Summary

Mixed mineral thixotropes  – MMTs – show advantages towards conventional organoclays and fumed silicas. The MMTs are able to form low-viscosity, pourable pregels and show easiest dispersibility. During handling they are low dusting due to their high bulk density. The preparation of coatings is improved in terms of handling and by shorter dispersion time. Even in solvent-free high solids, MMTs are suitable as they add only little viscosity to the application viscosity, but give a large increase in low-shear viscosity. MMTs give a very shear thinning, pseudoplastic thixotropy to e.g., unsaturated polyesters and 2-pack epoxies. This leads to improved application properties like better sag resistance and better storage stability. MMTs are a powerful easier-to-use alternative to fumed silicas.

MMTs are available from Southern Clay Products, Inc. under the trade name Garamite®.

This paper was presented at the Nürnberg Congress held during the European Coatings Show, Nürnberg, Germany, May, 2007 and organized by the Vincentz Network. See events@coatings.de.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Dr. Klaus Dziwok | Rockwood Clay Additives GmbH, Moosburg, Germany

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • A Novel Mixed Mineral Thixotrope Technology for Industrial Coatings

    See More
  • Southern Clay Products Gives Presentation on a New Mixed Mineral Thixotrope for Industrial Coatings

    See More
  • Modern Organic Thixotropes

    See More

Related Directories

  • Active Minerals International LLC

    Min-U-Gel® 400 & 500+ and Acti-Gel® 208 gellant attapulgite products provide syneresis control, thixotropic thickening, suspension and much more by creating a more uniform composite. One of the most economical, easiest-to-use and most stable rheology modifiers. High-brightness air-float kaolin products offer significant cost savings over water-washed kaolins.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing