Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Nanotechnology for Waterborne Paint Improvement

January 18, 2006
Biphor is a new family of aluminum phosphates or polyphosphates made by a patented wet chemistry process.8 It is a "green chemistry," zero-effluent product made under mild temperature and pressure conditions that do not create any environmental problems during the fabrication process. Due to its chemical nature, BIPHOR residues in the paint industry or in the final user location may be safely discarded in the environment as a fertilizer component.

(Click image for larger view)


What Is BIPHOR?

Biphor is a new family of aluminum phosphates or polyphosphates made by a patented wet chemistry process.8 It is a "green chemistry," zero-effluent product made under mild temperature and pressure conditions that do not create any environmental problems during the fabrication process.

Due to its chemical nature, BIPHOR residues in the paint industry or in the final user location may be safely discarded in the environment as a fertilizer component. It is produced as slurry as well as a dry powder. In both cases it is easily dispersed in water, forming stable dispersions that have stable rheological properties.

BIPHOR is completely different from existing aluminum phosphates or polyphosphates in many aspects.

  • It does not have a definite stoichiometry, thus it is better thought of as a crosslinked ionic polymer than as a salt.

  • Since the stoichiometry is not definite, various grades of BIPHOR can be prepared by changing the fabrication process, and thus the final product composition.

  • BIPHOR is made under very rigid pH control, and it is nearly neutral, thus avoiding environmental and toxicological problems.

  • It is also exempt from corrosion problems associated with some aluminum phosphates found in the marketplace and used in the transformation of iron oxides into iron phosphate in metal-protecting paints.

  • The non-stoichiometry, together with the non-crystallinity of BIPHOR (both slurry and powder) and the carefully controlled water content of dry BIPHOR powder, allow for easy swelling control that is essential for its performance, following the mechanism that will be described.

  • The nano-sized particles are easily dispersed and are stable towards settling, which is very important for making uniform paint dispersions with BIPHOR.

  • BIPHOR nanoparticles are strongly compatible with latex particles, by the mechanisms of capillary adhesion (in the dispersion drying stage) followed by ion-cluster mediated electrostatic adhesion (in the dry film). This compatibility is so high that bicontinuous networks are formed in many cases.

  • BIPHOR is also strongly compatible with many other particulate solids commonly used as paint fillers, such as the various silicates, carbonates and oxides found in formulated waterborne dispersions. This contributes to the cohesion and strength of the dry paint film.


(Click image for larger view)

Typical chemical composition data of the current product are shown in Table 1. Together with diffraction data (Figure 1), the infrared spectrum (Figure 2), electron and atomic force microscopy analysis (Figures 3 and 4) and thermogravimetric data (Figure 5) these results show that BIPHOR is a hydrous, non-crystalline and neutral aluminum phosphate made out of nano-sized particles. Particle size (in the slurry) is in the 200-2,000 nm range, as determined by dynamic light scattering.

How BIPHOR Works

To understand how BIPHOR performs within a drying paint film, it is interesting to compare it to the current industry-standard white pigment, titanium dioxide. A basic TiO2 waterborne paint is made out of a suitable latex dispersion and pigment particles. The latex particles are responsible for making a coalesced film filled with the pigmented particles, which are responsible for the film hiding power. Many additives are also used: inorganic fillers, which decrease the requirements of resin and pigment; coalescing agents that improve resin film formation; and dispersants and rheological modifiers that prevent pigment and filler caking, thus improving the paint shelf-life together with the rheological paint properties.

(Click image for larger view)

A typical dry paint film can thus be represented as shown in Figure 6. The pigment and filler particles are dispersed in the resin film. In this case, hiding power is largely dependent on the particle refractive indices and sizes. TiO2 is currently the standard white pigment because of its high refractive index and because of the absence of light absorption in the visible region.

A typical dry film of a paint formulated with BIPHOR is represented in Figure 7. There are many large differences compared to the previous case.

(Click image for larger view)

  • The film is not just a resin film; it is formed by enmeshed resin and aluminum phosphate. It is thus a nanocomposite film that combines two interpenetrating phases with different properties to achieve synergistic benefits concerning film mechanical properties and resistance to water and to other aggressive agents. This is a new concept for the paint industry but it is already largely used in the development of new, high-performance materials generally described as nanohybrids or nanocomposites.9

    (Click image for larger view)

  • Good film hiding power is obtained at lower TiO2 content because the film contains a large amount of closed pores that also scatter light. Moreover, if a TiO2 particle is adjacent to one of these voids, it will scatter much more than if it is fully surrounded by resin, due to the larger refractive index gradient. This creates a synergism between BIPHOR and TiO2 as far as the hiding power is concerned.

    (Click image for larger view)

    Application Tests

    In these tests, a standard market formulation of a semi-matte acrylic paint was chosen, and TiO2 was progressively replaced with BIPHOR. Water content and other paint components were adjusted as required. The majority of the modifications in the formula are related to a decreased use of thickener/rheology modifier, dispersant, acrylic resin and coalescing agent.

    Table 2 describes an example of one of the standard formulas used in this work, together with the corresponding BIPHOR formula. The standard formula in Table 2 is currently being used by one of the market leaders in the Brazilian architectural paint market.

    In the formula in Table 2, a replacement of 50% TiO2 (on a weight basis) was made, obviously keeping the opacity and whiteness conditions of the dry film. In addition, the other properties of BIPHOR as a rheological modifier and also as a film-structuring agent were explored.

    (Click image for larger view)

    Comparison between the two formulas shows that the basic intrinsic properties of BIPHOR will lead to additional cost reduction beyond that derived from the replacement of TiO2 pigment only. Moreover, these gains are obtained while producing excellent final performance in the applied paint film. Tables 3 and 4 show the evaluation results of the two architectural semi-matte acrylic paints referred to in Table 2, conducted by two independent laboratories. The formulation made by replacing 50% by weight of TiO2 with BIPHOR is comparable to the standard paint in gloss, reflectance, opacity, whiteness and yellowness. The appearance of dry drawn films formulated with BIPHOR (50%) and TiO2 (100%) is illustrated in Figure 8.

    Several field test applications were also made, and an example is shown in Figure 9. Some of these application tests have been monitored for quite some time now and they are revealing great color stability and resistance to chalking. This can be attributed to the complete photochemical inertness of BIPHOR (as compared to TiO2), bringing in a bonus for those paints formulated with BIPHOR.

    (Click image for larger view)

    Conclusion

    BIPHOR is now completing the development stage with outstanding results. The introduction of BIPHOR in waterborne paints leads to improved visual performance and durability at a reduced cost. c

    Acknowledgments

    FG acknowledges PADCT/CNPq for supporting the Instituto do Milênio de Materiais Complexos (Millenium Institute for Complex Materials).

    References

    1. Beppu, M.M; Lima, E.C.D.; Sassaki, R.M.; Galembeck, F. Self-opacifying aluminum phosphate particles for paint film pigmentation.; J. Ctgs. Technol. 1997, 69 (867): 81-88.
    2. Lima, E.C.D.; Beppu, M.M.; Galembeck, F.; Valente, J.F.; Soares, D.M. Non-crystalline aluminum polyphosphates: Preparation and properties. J. Brazilian Chem. Soc. 1996, 7 (3): 209-215.
    3. Beppu, M.M.; Lima, E.C.D.; Galembeck, F. Aluminum phosphate particles containing closed pores. Preparation, characterization, and use as a white pigment. J. Colloid Interface Sci. 1996, 178 (1): 93-103.
    4. Monteiro, V.A.D.; de Souza, E.F. ; de Azevedo, M.M.M.; Galembeck, F. Aluminum polyphosphate nanoparticles: Preparation, particle size determination and microchemistry. J. Colloid Interface Sci. 1999, 217 (2): 237-248.
    5. de Souza, E.F.; da Silva, M.D.C.V.M.; Galembeck, F. Improved latex film-glass adhesion under wet environments by using an aluminum polyphosphate filler. J. Adhes. Sci. Technol. 1999. 13 (3): 357-378.
    6. de Souza, E.F.; Bezerra, C.C.; Galembeck, F. Bicontinuous networks made of polyphosphates and of thermoplastic polymers. Polymer 1997, 38 (26): 6285-6293.
    7. Lima, E.C.D.; Beppu, M.M.; Galembeck, F. Nanosized particles of aluminum polyphosphate. Langmuir 1996, 12 (7): 1701-1703.
    8. Galembeck, F. "Produto e processo de fabricação de um pigmento branco baseado na síntese de partículas ocas de ortofosfato ou polifosfato de alumínio", Brasil, PI0403713-8, 2004.
    9. Giannelis, E.P. Polymer layered nanocomposites. Adv. Mater. 1996, 8 (1): 29-35.

    This paper was presented at ABRAFATI 2005, the 9th International Paint Congress, Sao Paulo, Brazil.
  • Share This Story

    Looking for a reprint of this article?
    From high-res PDFs to custom plaques, order your copy today!

    Recommended Content

    JOIN TODAY
    to unlock your recommendations.

    Already have an account? Sign In

    • pci1022-Kinaltek-Lead-1170.jpg

      A Novel Pigment Production Technology

      Following an extensive R&D program that demonstrated...
      Paint and Coating Pigments
      By: Jawad Haidar and Nitin Soni
    • pci global top 10

      2025 Global Top 10: Top Paint and Coatings Companies

      The following is PCI’s annual ranking of the top 10...
      Paint and Coating Market Reports
      By: Courtney Bassett
    • 2025 pci 25

      2025 PCI 25: Top Paint and Coatings Companies

      PCI's annual ranking of the top 25 North American paint...
      Paint and Coating Market Reports
      By: Courtney Bassett
    You must login or register in order to post a comment.

    Report Abusive Comment

    Manage My Account
    • eMagazine
    • Newsletters
    • Online Registration
    • Subscription Customer Service

    More Videos

    Sponsored Content

    Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

    close
    • wooden kitchen set and shelving
      Sponsored bySirca North America

      Leveraging Coatings to Meet ESG Goals in Manufacturing

    • man woodworking in workshop
      Sponsored byGemini Industries, Inc.

      Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

    Popular Stories

    Akzo, SW, Nippon Logos

    AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

    BASF SE Logo

    BASF Announces Strategic Business Sale

    AkzoSWNipponEndTalks

    Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

    POB-Point-and-Shoot

    PCI Buyers Guide

    Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

    Start your RFP

    Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

    Find Suppliers

    Events

    September 4, 2025

    N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

    ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

    September 15, 2026

    Coatings Trends & Technologies Summit

    The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

    View All Submit An Event

    Poll

    Longest-running laboratory experiment

    What is the longest-running laboratory experiment?
    View Results Poll Archive

    Products

    Automotive Paints and Coatings, 2nd Edition

    Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

    See More Products
    Inside the AI Shift in Coatings - See the article now

    Related Articles

    • Ford Looks to Nanotechnology for Performance, Fuel Economy Improvements

      See More
    • Innovation Drives Compact Paint Process for Waterborne Automotive OEM Coatings

      See More
    • LaFontaine Automotive Converts to Waterborne Paint System - Posted 6/10/08

      See More

    Related Products

    See More Products
    • Waterborne Polymers and Film Formation (Virtual Course - 7/23/26)

    See More Products

    Related Directories

    • Advancion Corp.

      Advancion Corporation (formerly ANGUS Chemical Company) is a leading global manufacturer of high-performance multifunctional additives, co-dispersants and stabilizers, and other specialty ingredients for waterborne paints, industrial coatings and indoor air quality improvement applications.
    • Serac Inc.

      Serac Inc delivers high-performance liquid filling machines, capping systems, and complete packaging lines for paints, chemicals, coatings, and lubricants. Competing with global leaders, Serac combines precision net-weight filling, advanced automation, and flexible line integration to handle high-viscosity and hazardous products. From pails to drums, our solutions maximize accuracy, safety, and efficiency. Based in the USA, Serac supports manufacturers across the Americas with engineered, reliable, and scalable industrial filling systems.
    ×

    Keep the info flowing with our eNewsletters!

    Get the latest industry updates tailored your way.

    JOIN TODAY!
    • RESOURCES
      • Advertise
      • Contact Us
      • Directories
      • Store
      • Want More
      • Manufacturing Division
    • SIGN UP TODAY
      • Create Account
      • eMagazine
      • Newsletters
      • Customer Service
      • Manage Preferences
    • SERVICES
      • Marketing Services
      • Reprints
      • Market Research
      • List Rental
      • Survey & Sample
    • STAY CONNECTED
      • LinkedIn
      • Facebook
      • Youtube
      • X (Twitter)
    • PRIVACY
      • PRIVACY POLICY
      • TERMS & CONDITIONS
      • DO NOT SELL MY PERSONAL INFORMATION
      • PRIVACY REQUEST
      • ACCESSIBILITY

    Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

    Design, CMS, Hosting & Web Development :: ePublishing