Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Preparation and Properties of UV-Curable Polyurethane Acrylate Resins for Metal Surfaces

By Devendra Agarwal, Sukhen Mistry, Jagbir Singh, Abhishek Srivastava
April 7, 2008
UV-curable coatings are a boon to the paint industry, as they not only reduce VOCs but also speed up production processes and provide protective, durable and attractive finishes. UV-curable polyurethane acrylates have been synthesized from polyester polyol (1,6-hexanediol, adipic acid and ethylene glycol), toluene diisocyanate and three types of reactive diluents i.e., ethoxylated phenol monoacrylate (EOPA), 1,6-hexanediol -diacrylate (HDDA) and trimethylolpropane triacrylate (TMPTA). In this paper several formulations of UV-curable polyurethane acrylate resins were used to study the effect of reactive diluents on performance properties. It was observed from the results that UV-cured polyurethane acrylate resin films on metal surfaces exhibit excellent gloss (60°), mechanical, and chemical- and stain-resistant properties.

UV-curable coatings are a boon to the paint industry, as they not only reduce VOCs but also speed up production processes and provide protective, durable and attractive finishes. UV-curable polyurethane acrylates have been synthesized from polyester polyol (1,6-hexanediol, adipic acid and ethylene glycol), toluene diisocyanate and three types of reactive diluents i.e., ethoxylated phenol monoacrylate (EOPA), 1,6-hexanediol -diacrylate (HDDA) and trimethylolpropane triacrylate (TMPTA). In this paper several formulations of UV-curable polyurethane acrylate resins were used to study the effect of reactive diluents on performance properties. It was observed from the results that UV-cured polyurethane acrylate resin films on metal surfaces exhibit excellent gloss (60°), mechanical, and chemical- and stain-resistant properties.

Introduction

Light-induced polymerization of multifunctional monomers is one of the most efficient methods to rapidly synthesize highly crosslinked polymer networks. A liquid resin can be transformed within seconds into a solid polymer totally insoluble in organic solvents and very resistant to heat, chemical and mechanical treatments.1,2 This technique has been applied commercially in printing, thin film coatings and adhesives.3,4

Photo-curable formulations usually consist of multifunctional monomers, reactive diluents, oligomers and photoinitiators, which generate reactive species on UV exposure.5,6 Typically it is a segment of polyurethane oligomer tipped with acrylic functionality such as 2-hydroxyethylacrylate (HEA) or 2-hydroxyethylmethacrylate (HEMA).

The reactive diluents are acrylic monomers that are added to modify properties and to reduce viscosity of the precursor liquid.

The acrylated urethanes ideally combine the abrasion resistance, toughness, tear strength and good low-temperature properties of PU with the superior optical properties and weatherability of polyacrylates.7-9 The reactive diluent phase is more compatible with the hard segments of polyurethane rather than the soft segments, due to similar polarity and hydrogen bonding formation between the urethane NH and acrylate carbonyls.10

This paper considers the preparation and properties of UV-curable polyurethane acrylates. The NCO-terminated polyurethane prepolymers were synthesized from toluene diisocynate (TDI) and polyester polyol followed by tipping with 2-hydoxyethylmethacrylate (HEMA). In addition, three types of reactive diluents having mono-, di- and tri- functionality were used in different concentrations. A series of coating compositions having PU acrylate and reactive diluents were prepared, and their mechanical, chemical, optical and stain-resistant properties studied.

Experimental

Reagents
TDI (an 80/20 mixture of 2,6 and 2,4 isomers) was obtained from BASF and Narmada Chematur. The purity was 98% and was used as such. Laboratory reagent (LR)-grade adipic acid, 1,6-hexanediol, ethylene glycol, 2-hydoxyethylmethacrylate (HEMA) and hydroquinone of M/s Thomas Baker, Mumbai, were used. Reactive diluents were procured from M/s Cognis, Thailand, and photoinitiators were procured from M/s Ciba chemicals.



Polyester Polyol Synthesis
Initially ethylene glycol, adipic acid and 1,6-hexanediol were placed in a three-neck, round-bottom flask in the molar ratio of 1.6 : 3.4 : 4.0 respectively. The esterification reaction was catalyzed by adding dibutyl tin oxide (0.1%) as a catalyst. The temperature was maintained at 140 – 150 °C. An inert atmosphere was maintained by blanketing the reaction mixture with nitrogen. Acid and hydroxyl values (Figures 1 and 2) of the resin were checked at fixed time intervals.

Urethane Acrylate Synthesis
The reaction flask was charged with 2.2 moles of TDI under dry nitrogen gas at 50 °C; a blend of 2.4 moles of HEMA with hydroquinone (50 ppm) was added continuously over a period of one half hour while maintaining a maximum temperature of 60 °C. After the addition was complete, the reaction mass was kept at 60 °C for half an hour to assure the complete conversion of the hydroxyl group of HEMA.



Polyurethane Acrylate Synthesis
The temperature of the reaction flask containing urethane methacrylate precursor was maintained at 50 °C, and a mixture of hydroxyl functional polyester polyol and hydroquinone (50 ppm) was added over a half-hour period. An inert gas atmosphere was maintained in the reaction flask by blanketing dry nitrogen gas throughout the reaction period. The reaction completion was determined by monitoring the hydroxyl value of the resin at definite intervals (Figure 3).

Evaluation and Characterization

An FTIR spectrum of polyurethane acrylate resin was recorded using a NaCl cell on a Perkin-Elmer 1750 FT-IR spectrophotometer. Molecular weight of the resin was obtained by GPC (model HPLC 600, RI detector on a styragel column) using polystyrene as a standard and THF as an eluent. The hydroxyl value of the resin was determined by titration (Table 1).



Coating Sample Preparation
Coating samples were prepared by using resin, hydroxylcyclohexyl phenyl ketone (HPCK, 25% by wt.) and reactive diluents in different ratios. The sample designations are given in Table 2.



Sample Characterization
Coating sample viscosities were determined by a Brookfield Viscometer, and refractive index was determined by a Mettler Refractometer (Toledo RE 40D). Data is shown in Table 3.

Curing
The UV-cured PU-acrylate films were prepared by applying the various coating formulations on mild steel panels using a bar applicator. The dry film thickness was maintained at ~12 microns with the help of a film applicator for the evaluation of various mechanical and chemical resistance properties. The panels were then exposed to a UV lamp chamber (GT Ultra Cure, 120 w/cm) maintained as follows.
  • UV dryer type : GT Ultra Cure 250
  • Curing width: 250 mm
  • Bulb type: UV (medium pressure)-GT 250 pure
  • Transparent: 120 watt/cm
  • Silica Quartz
  • Air cooling: 100 mm
  • Operating voltage: 440 volts 3 phase A.C.
  • Speed: 50 cycles
  • Power consumption: 120 w/cm for UV


Results and Discussion

Infrared Analysis
Figure 4 shows the IR spectrum of the PU-acrylate resin. A weak band 1180 cm-1 is attributed to C-N stretching. A band at 1651 cm-1 confirms the formation of the urethane group. A band at 1534 cm-1 is attributed to N-H deformation. A strong band at 1735 is from the acrylate ester carbonyl group present in PU-acrylate resin. A strong band at 2963 cm-1 is believed to be due to C-H stretching and a strong band at 3345 cm-1 is thought to be arising from –OH stretching, due to residual hydroxyl group present in the resin. Moreover, the absence of any band at 2270 cm-1 in the spectrum confirms that unreacted NCO groups are not present.



Molecular Weight
Figure 5 shows the molecular weight distribution of the PU-acrylate resin. It is clear from the figure that the synthesized resin is a low-molecular-weight resin.

Characterization of Coating Films
Various coating formulation panels were cured in the UV chamber and tested for different mechanical and chemical resistance properties, as per the following test methods: gloss at 60° (ASTM D 523-99); scratch hardness (ASTM D 5178); pencil hardness (ASTM D 3363-00); chemical resistance (EN: 438-2:1991) and stain resistance (ISO-4211).



Scratch Hardness
Scratch hardness is one of the important mechanical properties required for a coating to fulfill its protective role. The damage caused by a scratch on a cured surface may lead to a change in the gloss properties of the coating or it may be severe enough to cause deformation and finally induce cracking in the coating. Scratch hardness was determined using an automatic scratch hardness tester having a hardened steel hemispherical point of 1 mm diameter as a scratching needle. Results are shown in Table 4.

It is clear from the data that films having a higher concentration of TMPTA, i.e., sample A, have high scratch hardness due to maximum extent of crosslinking of the monomer.



Cross-Hatch Hardness
Cross-hatch was measured by using a cross-cut adhesion tester. The tester consists of a die made up of 9 parallel blades, 1/16 inches apart and 1 mm in length. The die is pressed into the panel in two directions at right angles to each other. A strip of self adhesive was staked over the pattern, left in contact for 10 seconds and stripped rapidly by pulling the tape back on itself at an angle of ~120°. The test was rated good if 5% of the squares were removed. All the coating samples had good cross-hatch hardness properties (Table 5).



Pencil Hardness
In the test, a strip is drawn under a pencil until a hardness grade is reached that will scratch the surface. The coating film is then assigned a hardness value such as H, 2H, 3H, etc., signifying the hardness grade. Coating films of TMPTA showed maximum hardness due to higher functionality that led to a maximum degree of crosslinking (Table 6).



Gloss
Gloss was measured using a Triglossometer (Sheen). After watching the films from a 60° angle, it was observed that all the coating films had good gloss. Coating films of EOPA showed maximum gloss (Table 7).



Flexibility
Flexibility testing was carried out on a ¼-inch Mandrel bend tester. Films of all coatings compositions were flexible enough to pass through the Mandrel (Table 8).



Chemical Resistance
The coatings samples were tested for their chemical resistance properties. The results of the tests are shown in Table 9.

Distilled Water Resistance
Coating films exhibit good resistance when exposed to distilled water. Samples, which have a high percentage of TMPTA, showed better resistance (Table 9).



Acid Resistance
Films of EOPA and HDDA were affected by acid solution due to poor crosslinking of monomers. Samples of TMPTA showed excellent resistance against acid solution (Table 9).



Alkali Resistance
To examine alkali resistance, coating films were exposed to 0.1 N NaOH solution. Films of TMPTA showed better resistance due to high functionality of the monomer that leads to maximum crosslinking (Table 9).



Stain Resistance
In accordance with ISO-4211, panels were coated and allowed to cure in the UV chamber. The coated panels were kept at room temperature for 24 hrs. Droplets of tea, coffee and hot water were pipetted onto the films and covered with a glass cup for 24 hours to prevent evaporation. The films were carefully cleaned, and the film’s surface was analyzed (Figures 6 – 8).

Conclusion

UV radiation was effectively used to cure PU-acrylate resins in the presence of reactive diluents to obtain coatings for metal surfaces having excellent mechanical and chemical properties. UV-cured metal surfaces also exhibit excellent stain resistance properties. Coating properties were greatly affected when the reactive diluents were incorporated in the resin. At higher concentration of reactive diluents, gloss and scratch hardness increases. TMPTA showed better mechanical and chemical properties than EOPA and HDDA due to higher functionality, which leads to a maximum degree of crosslinking, providing excellent mechanical and chemical properties. Therefore these coatings can be used as protective coatings for metals and can also reduce VOC and hazardous air pollutants.

For more information, e-mail abhishekhbti27@gmail.com or dahbti@rediffmail.com.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Department of Oil & Paint Technology, Harcourt Butler Technological Institute, Nawabganji, Kanpur, India
Department of Oil & Paint Technology, Harcourt Butler Technological Institute, Nawabganji, Kanpur, India
Jubilant Organosys Ltd., Noida, Uttar Pradesh, India
Department of Oil & Paint Technology, Harcourt Butler Technological Institute (HBTI), Nawabganj, Kanpur, India

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • UV-Curable Polyurethane Acrylate Dispersions Compared to 100%-Solids

    See More
  • Radiation-Cured Coatings for Metal Surfaces

    See More
  • Valspar.jpg

    New Options for Wood and Metal Surfaces

    See More

Related Products

See More Products
  • Handbook of Adhesives and Surface Preparation

  • thin film.jpg

    Thin Film Coatings Properties, Deposition, and Applications

  • nanostructuredthinfilms.jpg

    Nanostructured Thin Films and Coatings: Mechanical Properties

See More Products

Related Directories

  • Keyland Polymer UV Powder LLC

    Keyland Polymer develops, formulates, manufactures and sells UV cured powder coatings for wood, plastic, metal, composites, and other substrates. Keyland Polymer has a complete resin synthesis lab with global reach and distribution capabilities for the development, formulation, testing, and manufacturing of UV/EB curable solid resins.
  • Epic Resins

    Epic Resins is a formulator of one- and two-component epoxy and polyurethane adhesives for use with natural, nylon, polyester, olefin and vinyl filaments. We have served the paint applicator industry with a complete line of standard products, as well as the ability to custom formulate. ISO 9001 and ISO 14001 Certified.
  • BASF Corp., Dispersions, Resins & Additives

    BASF offers a strong portfolio of industry-leading additives for the Coatings Industry to deliver eco-efficient solutions that meet performance requirements. The BASF Performance and Formulation additives portfolio encompasses a technology base of dispersing agents, wetting agents and surface modifiers, defoamers, rheology modifiers, film forming agents, antioxidants, light stabilizers and UV absorbers.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing