Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Rheological Aspects of Carboxymethyl Cellulose Acetate Butyrate (CMCABTM) in Waterborne Coatings

June 5, 2003
Figure 1 / CAB Strengths
Water-dispersible carboxymethylcellulose acetate butyrate (CMCAB[TM]) cellulose ester is the latest generation of mixed cellulose esters developed for use in aqueous coating formulations. In waterborne coatings, it offers reduced dry-to-touch times, improved metallic flake orientation in metallic basecoats, and improved flow and leveling characteristics. Like CAB in solventborne systems, CMCAB achieves these effects through near-Newtonian rheology, high Tg, and a steep viscosity/solids relationship.

Cellulose ester technology has been used in coatings since 1890 when cellulose nitrate (NC) was found to be useful as a coatings resin. Cellulose acetate (CA) and mixed cellulose esters such as cellulose acetate butyrate (CAB) and cellulose acetate propionate (CAP) were developed in the 1930s as a less flammable alternative to nitrate-based coatings for military aircraft. Cellulose esters can be used as binder resins or as additives to coatings to provide application properties and resist film defects.

Figure 2 / CMCAB and CAB Comparison
Cellulose esters provide unique properties to coatings based on three inherent properties: high Tg, a steep viscosity-solids relationship and near-Newtonian rheology. Figure 1 illustrates the benefits achieved by coatings through each of these properties. The high Tg of cellulose esters contributes rapid dry-to-touch, block and print resistance, and hardness development. The exponential viscosity-solids relationship contributes metallic flake control, redissolve resistance and anti-sag properties. Newtonian rheology contributes flow and leveling, and resistance to defect formations such as craters and pinholes.

Figure 3 / Comparison of Evaporation Rates for Water- and Solventborne Coatings at Room Temperature
Mixed cellulose esters are high-molecular-weight, high-Tg, rigid rod-type polymers derived from cellulose. The anhydroglucose repeat unit of cellulose is connected by a ?-1-4 glycosidic linkage giving cellulose more rigidity than other glycosidic polymers having alternative linkages. Commercially, the hardness, Tg and compatibility are controlled by the acetyl/butyryl (or propionyl)/hydroxyl ratios of the substituents in addition to the molecular weight of the polymer chain.1

Figure 4 / Log Viscosity vs. Log Shear Rate
The highly lipophilic nature of cellulose acetate butyrate without modification makes CAB unsuitable in aqueous systems where the balance between flow and sagging is particularly important. CMCAB cellulose ester is a cellulose mixed ester with sufficient acid groups to allow neutralization and subsequent dispersion in water while maintaining good hydrolytic stability. The acid number is approximately 60, making the cellulose ester easily soluble in solvents and dispersible in water when neutralized by a base. The acetate and butyrate esters contribute substantial lipophilicity. CMCAB cellulose ester brings to waterborne coatings many of the same benefits attributable to the three inherent properties (high Tg, steep viscosity-solids relationship, and near-Newtonian rheology) that other mixed esters bring to solventborne coatings. The effects brought about by the rheology and viscosity-solids properties in waterborne coatings are especially interesting.

Figure 5 / Zero Shear Viscosities as Paints Dry at Different Rates at Room Temperature
The hydrophilic, water-dispersible CMCAB cellulose ester is shown in comparison to CAB in Figure 2. Note the carboxymethyl group on the CMCAB. In reality, it is present only at every 2-3 repeat units.1

In waterborne coatings systems, the percent solids increases more slowly due to the slow evaporation rate of water (see Figure 3), especially at higher humidity. This slow evaporation makes it difficult to prevent a waterborne paint from dripping or sagging if it exhibits good flow and leveling. Avoiding these properties requires careful adjustments of the rheological profile of the coating. Rheology-control agents such as alkali-swellable thickeners, associative thickeners and clays are used to build viscosity rapidly to prevent the coating from dripping off vertical substrates. By using these agents, the viscosity increases rapidly due to a decrease in shear rate instead of relying on a rapid increase in solids and viscosity due to evaporation. Rheological additives that prevent dripping also aid in keeping the pigments dispersed. However, the elasticity introduced by such additives can be detrimental to flow and leveling and can propagate other film defects. To compensate for some of these problems, other additives are then needed to reduce the surface tension of the fluid in order to facilitate flow and leveling.2-3 The balancing act between good flow and leveling and sag control can be difficult to achieve.

Figure 6 / Viscosity vs. Shear Rate -- Waterborne Basecoats
CMCAB cellulose ester has been shown to be useful with other aqueous rheology modifiers, flow and leveling agents, or sag-control agents to maximize flow and leveling without hurting sag resistance at approximately 2-7% of the total coating resin content. At even higher levels of addition, it may be used as the sole additive.1

To use CMCAB cellulose ester in a waterborne coating formulation, it must first be dissolved in a suitable solvent system such as ethylene glycol butyl ether. In order to make an aqueous dispersion, this solution then needs to be partially neutralized with a suitable base such as an organic amine, diluted with water to form a dispersion, and then further neutralized with base to achieve the desired pH. The CMCAB solution or dispersion can then be added to the coating.

The acid number of the CMCAB cellulose ester is 60; to obtain a stable aqueous dispersion, only some of the acid functionality should be neutralized. Complete neutralization of the acid on the CMCAB may result in partial hydrolysis of the ester, leading to viscosity changes and precipitation. The method outlined is based on an ethylene glycol monobutylether solution and results in a 15% neutralization of the acid functionality on the CMCAB. Other solvents may be used to dissolve the CMCAB cellulose ester ranging from ketones, esters, and various glycol ethers as appropriate.

Figure 7 / Comparisons of Spray Patterns of a Waterborne Clear Containing CMCAB Cellulose Ester (Top) and a Waterborne Clear Containing Alkali-Swellable Thickener
Previous studies and anecdotal reports indicate that CMCAB cellulose ester affects application and drying behavior of waterborne systems in a manner similar to the effect of cellulose esters on solvent borne systems. This article looks at effects of CMCAB cellulose ester on spray atomization and drying behavior of waterborne coating systems.

Figure 7b

Experimental Materials

CMCAB cellulose ester dispersions were prepared by dissolving 20 g CMCAB 641-0.5 into 30 g ethylene glycol monobutylether on a high-shear mixer. Fifty g of water containing 0.5% dimethyl ethanolamine was added slowly with rapid mixing.

Waterborne basecoats were prepared by dispersing Silberline E3053 Aluminum pigment paste in an acrylic dispersion (Eastman Jagotex EM325) and adding CMCAB dispersion or Borchigel 75N polyurethane thickener (Borchers) to achieve a P/B of 0.15. Basecoat pH was adjusted to 8.5 and basecoat viscosity was adjusted to 15.5 sec DIN 4.

Commercial waterborne basecoats were obtained from the manufacturers.

Waterborne clears were prepared by mixing Paraloid WR97 (Rohm and Haas) and Cymel 327 (Cytec) at a solids ratio of 50/27. The pH was adjusted to 8.5 with AMP-95 (Angus) and BYK 380 was added at 0.15%. This was further modified with either 10% CMCAB on solids or 3% ASE-60 (Rohm and Haas) on solids.

Figure 8 / Comparisons of Film Smoothness of a Waterborne Clear Containing CMCAB (Top) and a Waterborne Clear Containing Only Alkali-Swellable Thickener as Rheology-Control Agent

Measurement Techniques

The viscosity curves in Figure 4 were obtained using a Haake RV-20 viscometer equipped with a Couette fixture. To retrieve data at lower shear rates, shown in Figure 5, another rheometer was used. The steady shear viscosity and dynamic viscosity were measured on a Rheometrics Dynamic Stress Rheometer (DSR) at 25 deg C. The steady shear viscosity was measured using a Couette fixture of 32 mm diameter cup and 29.5 mm diameter bob with 44 mm length. The zero shear viscosity was estimated from the Newtonian plateau at the shear rates around 10-3 sec-1 or lower. The dynamic frequency data were measured using 40 mm diameter parallel plates with 0.5-1 mm gap under a 10 dyne/cm2 stress set.

Figure 9 / Frequency Sweeps Showing Dynamic Viscosity (Eta*), Viscous Modulus (G"), and Elastic (G') for Two Commercial Waterborne Basecoats and for a CMCAB Basecoat

Results

Figure 4 shows the near-Newtonian nature of a CMCAB cellulose ester water dispersion compared to a solventborne CAB system and pure Newtonian rheology. The rheology change of the coating material upon application to the surface is of great interest. Figure 5 demonstrates that the increase in viscosity of a CMCAB-based water dispersion during spray application is faster than that of a waterborne system without CMCAB cellulose ester. It should be noted that the faster viscosity increase of the CMCAB system is not due to faster solvent evaporation but due to faster increase in viscosity and elasticity during drying. Figure 6 compares the viscosity vs. shear rate behavior of a waterborne basecoat containing CMCAB cellulose ester to the behavior of two commercial waterborne basecoats. The CMCAB basecoat exhibits near-Newtonian behavior.

Figure 9b
The near-Newtonian rheology and the lower viscosity of CMCAB-based waterborne system should result in different affects on application properties. Spray patterns of waterborne systems with and without CMCAB cellulose ester were photographed for comparison purposes. Figure 7 shows that the spray pattern of the waterborne system containing CMCAB cellulose ester is fuller with a smaller droplet size than the waterborne system without CMCAB.

Figure 9c
The near-Newtonian nature of CMCAB cellulose ester also promotes flow of the droplets immediately upon hitting the substrate when compared to the orange peel effect caused by the elasticity of an alkali-swellable thickener. This is demonstrated in Figure 8, which compares the surface drying of the same waterborne clears from Figure 7 immediately after application on top of a blue metallic basecoat. The coating system with CMCAB (top) has a smooth surface immediately after application while the coating without CMCAB (bottom) shows orange peel develop immediately after application.

Figure 9 shows the dynamic mechanical behavior of a CMCAB cellulose ester system in comparison with two commercial basecoats. The basecoat containing CMCAB shows very different viscosity and elasticity behavior than the two commercial basecoats.2-3 In particular, the elasticity (G') of the CMCAB system is very much lower than the other two basecoats.

Conclusion

CMCAB cellulose ester appears to exhibit unique rheological properties in waterborne coatings. Comparisons of rheology behavior and elasticity measurements of a waterborne coating containing CMCAB cellulose esters to waterborne coatings using other rheology control agents indicate that CMCAB provides a different rheology control mechanism. Spray patterns and flow of coatings material immediately on application also support a unique rheology control mechanism. Thickening behavior as a function of solids increase and near Newtonian behavior in the film supports observations of good flow and leveling combined with sag resistance.

This article is based on a paper presented at the 30th International Waterborne, High-Solids, and Powder Coatings Symposium February 26-28, 2003, in New Orleans. Symposium sponsored by The University of Southern Mississippi School of Polymers and High Performance Materials.

For more information, contact Jonathan E. Lawniczak, Eastman Chemical Company, P.O. Box 431, Kingsport, TN 37662.

References

1Posey-Dowty, J.D.; Seo, K.S.; Walker, K.R.; Wilson, A.K. (2002) "Carboxymethylcellulose Acetate Butyrate in Water-based Automotive Paints," Surface Coatings International, Vol 50, 303-08.
2 Osterhold, M. (2000) "Rheological Behavior of Automotive Paint Systems: Modern Characterization Methods with Good Correlations to Observable Effects." European Coatings J., Vol. 4/00 18-33.
3 Boggs, L.J.; Law, D.; Taniguchi, H. (1998) "Rheological Properties and Aluminum Flake Orientation in Waterborne Automotive Coatings," International Waterborne, High-Solids. And Powder Symposium: New Orleans, February 18-20, 1998.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • Off-Diagonal Effects of Alkanolamines in Waterborne Coatings

    See More
  • The Use of Aqueous Pre-Dispersed Fumed Silica to Improve Film Formation in Waterborne Coatings

    See More
  • Study Predicts Rise in Waterborne Coatings in the Protective and Specialty Markets

    See More

Related Products

See More Products
  • Adhesion, Surface Aspects & Coatings Defects (Virtual Course - 10/22/26)

  • durability.jpg

    Increasing the Durability of Paint and Varnish Coatings in Building Products and Construction 1st Edition

  • Handbook of Adhesives and Surface Preparation

See More Products
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing