Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Trimethylol Propane Monoallyl Ether as Hydroxyl-Functional Co-Monomer

By Mircea Manea, Sri Pauliana, Mayke Winarti
October 1, 2008

The interest for hydroxyl-functional acrylic resins as a component in polyurethane coatings has increased not only because of improved performance through crosslinking, but also because of higher non-volatile content. Hydroxyl functionality may be introduced in acrylic resins by the use of a hydroxyl-functional monomer. However the range and latitude of choice are limited as commercial monomers have a limited portfolio (Table 1).

Hydroxyl Functionalization of Acrylic Backbones

Another approach is functionalization of the acrylic backbone, in most cases acid functional, to a hydroxyl-functional one, in which case the hydroxyl functionality is a secondary group (Figure 1).

In this case the oxirane derivative may be anything from propylene oxide, Cardura E10 or any glycidylated acid, or an epoxy alpha-olefin.1 Primary hydroxyl groups may be obtained by anhydride opening on the backbone with a diol (Figure 2).

The approach allows a larger latitude of formulation, targeting a lower or higher mobility of the hydroxyl group, related to the length of the R’ chain. In most cases propylene glycol, ethylene glycol, 1,6-hexane diol and 1,4-butane diol may be used but also cyclohexane dimethanol, 1,4- or  a commercial blend with the 1,3- isomer. However the limitation of the method resides in the risk for looping and interchain esterification that may lead to gellation. This approach also increases the acid functionality at the same rate as the hydroxyl functionality.



Another interesting approach described in the literature is the reaction of a solventborne acrylic backbone bearing pendent glycidyl groups that are further reacted with a hydroxyl amine to yield a hydroxyl-functional acrylic (Figure 3). This approach,2,3 although very interesting, is limited in application due to the potential oxidation of the tertiary amino group leading to severe discoloration.

Trimethylol Propane Monoallyl Ether as Hydroxyl-Functional Co-Monomer

The present work introduces a new hydroxyl-functional monomer having the benefits of lower equivalent weight, higher flexibility, lower viscosity due to aliphatic substituent, and the same mobility and reactivity of the hydroxyl groups. The monomer is trimethylol propane monoallyl ether, or TMPME (Figure 4).

Although the allyl group may show lower reactivity in the polymerization process, no experiment in the given conditions exhibited free monomer. Some standard formulations are presented in order to assess the properties of TMPME as monomer as well as the benefits of this building block in acrylic polyols.

Experimental

Table 2 shows the standard formulations used to assess the properties of TMPME as functional monomer in acrylic polyols compared to standard hydroxyl-functional monomers. All formulations have been chosen to have the OH number in the same range and the ratio of styrene/butyl acrylate by weight to be 2/1.

Syntheses were carried out in a nitrogen atmosphere at 150 ºC simultaneously dropping the monomer blend and initiator (in xylene) over a 5-hour period. Only Formulation 4 used a xylene/n-butanol solvent blend in order to tackle the high viscosity during the synthesis and was lowered in non-volatile content at the level of 65%.

The experiments using TMPME as hydroxyl-functional monomer were carried out using the TMPME in a solution of xylene in which, at reflux, the radical initiator xylene solution and the styrene and butyl acrylate blend were loaded simultaneously drop-wise over a period of 5 hours (in similar conditions as for all other hydroxyl functional monomers).

The complete reaction of TMPME was confirmed by the absence of the double bond in the IR spectra and by the attempt to extract the free monomer with water from a diluted polymer sample. All water extracts had a zero non-volatile content showing that the TMPME had been completely reacted. The residual initiator was destroyed by maintaining the polymer at 150 ºC under nitrogen flow and verified over time using kalium iodine (KI) solution.



The acrylic binders were tested for reactivity by using them in formulations with polyisocyanate crosslinker and melamine resin in both air and respectively oven-cured compositions. The reaction ability of the hydroxyl group was evaluated by reaction with fatty acids. This approach was considered in an attempt to produce high-solids resins having an acrylic backbone. This choice is interesting because of using a co-polymer backbone having a low-molecular-weight distribution and pendent oxidative drying groups from fatty acids.



The narrow molecular weight distribution of a higher-molecular-weight polymer should theoretically secure a lower viscosity. The high molecular weight of the backbone is responsible for the performance of the polymer, but the presence of very high molecular weight strongly increases the viscosity (Figures 6 and 7).4



Although the acrylic backbone has higher molecular weight, the presence of the pendent fatty acids shields the higher Tg of the backbone and at the same time reduces the availability of H bonding between polymer chains.

Isocyanate Curing of Hydroxyl-Functional Copolymers

The hydroxyl-functional acrylic binders were cured at room temperature with polyisocyanate Desmodur 3790®. The curing performance is shown in Figure 8. All trials were carried out at a ratio of 1:1 hydroxyl to isocyanate.



Curing was performed at room temperature without any catalyst addition. Formulation 8 exhibited a shorter pot life as a result of the catalytic activity of the existing small amount of carboxyl groups (acid number = 10 mg KOH/g) (Figure 9).

Formulation 4 has not been tested following the addition of n-butanol for high-viscosity reduction. The hardness is comparable for all copolymers, but the pot life is different. 2-HPMA has a long pot life that may be explained by the presence of secondary hydroxyl groups. The copolymer containing 2-HEA has a lower reactivity due to the fact that the hydroxyl group, although a primary group, is too close to the polymer backbone, thus presenting lower mobility. The copolymer containing hydroxyl groups from the 4-HBA has a shorter pot life, probably due to the higher mobility of the hydroxyl groups positioned at a longer distance from the backbone. The copolymers functionalized from TMPME may suffer from a combined effect from the vicinity and steric hindrance; as expected, one of the two hydroxyl groups in position 1,3 should react first, and then the second group at a slower rate, being already trapped in the newly generated network.

Curing with Melamine Resins

Curing of the hydroxyl-functional poly(styrene-acrylic) resins was performed at  140 ºC for 35 minutes. The melamine resin used for cure is a blend of melamine and toluene sulfonamide at a molar ratio of approximately 10:1 by mol. The application was done at a constant non-volatile content of 60% and a ratio of styrene-acrylic resin/amino resin 68/32 calculated on solids (Table 3).



Figure 10 shows that using TMPME as monomer gives the best flexibility-hardness correlation. Formulation 8 containing TMPME  emphasizes the catalytic effect of the existing carboxylic groups in the backbone, as introduced by the acrylic acid.

Alkyd Resins with Copolymer Backbone

Table 4 lists the alkyds synthesized using the poly(styrene-acrylic) hydroxyl-functional backbones. As expected, the viscosity of the copolymer backbone esterified with fatty acids is lower than the viscosity of the starting (intermediate) copolymer, confirming the assumption that 1) the reduced hydroxyl functionality and 2) the shielding offered by the fatty acids acting as built-in solvent, both have strong effects in viscosity reduction. The viscosity of the alkyd resulting from a styrene-acrylic backbone modified with TMPME is lower than the alkyd from the backbone corresponding to the other hydroxyl functional monomer 2-HPMA. This may be explained by the presence of the ethyl group shielding the ester groups on the polymer backbone and hindering hydrogen bonding. The ethyl group from the TMPME has the effect of a ‘built in’ solvent, acting in viscosity reduction with a larger effect compared to the methyl group in the 2-HPMA, and also exhibiting a plasticizing effect. This is also reflected in the hardness of the alkyd as the ethyl group is reducing the physical drying lowering the Tg of the backbone.

Conclusions

The present work recommends the use of TMPME as a hydroxyl-functional monomer for vinyl co-polymer backbones. The differences in reactivity for hydroxyl-functional co-polymers may be related to the mobility of the hydroxyl group, which is the distance between the functional group and the co-polymer backbone. The drying performance of hydroxyl-functional copolymers with amino resins and isocyanates is perfectly comparable, thus recommending the use of TMPME as a good replacement for sophisticated monomers. The use of TMPME always yields lower viscosity co-polymers when compared to the other existing options. Also the use of TMPME may lead to alkyd resins having a high non-volatile content and improved performance due to the high-molecular-weight backbone at a reasonable cost.

Acknowledgment
The authors would like to thank Perstorp Specialty Chemicals (TMPME), Bayer AG, KOWA (4-HBA), Indochemical Citra Kimia (2-HEA, 2-HPMA) and Justus Kimia Raya (Styrene, Butyl acrylate), Arizona Chemicals (TOFA), for supplying the samples used in this experimental work. The authors are also thankful to Hendra Adidarma, Kris Adidarma, and Sugianto Effendi for making possible this investigation.

For further information, e-mail mircea.manea@telia.com.<

Bibliography

1.            Holmberg, K. High solids alkyd resins, ISBN 0-8247-7778-6.
2.         Manea, M., et al, High solids alkyd strategy, Paint and Coatings Industry, July 2007.
3.            DE3822995.
4.            EP047061.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Consultant, PT. Propan Raya Group, Indonesia
PT. Alkindo Mitraraya, Tangerang, Banten, Indonesia
PT. Alkindo Mitraraya, Tangerang, Banten, Indonesia

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • Novel Path to Hydroxyl-Functional Emulsions

    Novel Path to Hydroxyl-Functional Emulsions

    See More
  • Polyurethane Dispersion Process by Hydrophilic Monomer Dissolution

    See More
  • aerial top view of harvesting truck and field

    Biobased 1,5 Pentanediol as a Low-Emission and High-Performing Monomer

    See More

Related Products

See More Products
  • nanostructured.jpg

    Nanostructured Thin Films and Coatings: Functional Properties

  • pci july 2019

    PCI July 2019 Issue

  • pci may 2020

    PCI May 2020 Issue

See More Products

Related Directories

  • Kowa American Corp.

    Offers the widest selection of specialty and UV-curable monomers, including Acrylates, Methacrylates, Acrylamides, vinyl ethers, Thiol-ene and cycloaliphatic expoxides. Organic microspheres for matting agents/abrasion resistance. VOC-exempt solvents DMC and PCBTF. Low viscosity & waterborne HDI specialty resins. Low-MW acrylic polymers with silyl, hydroxy or carboxy functionalities used as reactive liquid polymers.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing