Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Hydroxy Ethyl Fatty Amide Effect on the Perfomance Properties of Polyesteramide Resins Based on Acrylic Copolymers

By Devendra Agarwal, Sukhen Mistry
February 1, 2009


One of the major pollutants emitted by a surface coating is organic solvent used during processing and application. Hence, efforts have been made to develop alternative technologies that minimize the use of organic solvents in surface coatings. These include the use of coating curing agents derived from vegetable oils, which have been directly used to obtain coating films. Since these oils, by themselves, cannot directly meet the desired film properties, a number of oil modifications have been proposed such as alkyd, epoxy, polyesteramide, polyurethanes, polyurethaneamide, etc.1-10 The polyesteramide resins hold considerable application scope in the coatings field.11 A number of polyesteramides have been developed from different oils e.g., dehydrated castor oil,12 pilu fat,12 argemone,13 linseed14, etc. The presence of repeating units of ester (-COOR) and amide (-NCOR) in the polymeric chain of polyesteramide (PEA) improves the ease of application, thermal stability, chemical and water resistance, and causes faster drying and enhanced hardness over normal alkyds.15 These polyesteramides have shorter curing times at elevated temperature, while considerably longer times at room temperature.

In the present study, an acid-functional acrylic copolymer has been synthesized using butyl methacrylate and maleic anhydride. In addition, the hydroxyl ethyl fatty amide of castor oil has also been synthesized and used as a curing agent for the acid-functional acrylic copolymer to form polyesteramide resins. The effect of crosslinking agent on the acrylic copolymers was examined. A series of coating compositions with varying amounts of acrylic copolymer and hydroxyl ethyl fatty amide were prepared, and their mechanical, optical and chemical resistance properties studied.

Experimental
Reagents
Castor oil was procured from a commercial manufacturer. Maleic anhydride, butyl methacrylate (BMA), diethanolamine, zinc oxide, methanol, xylene, acetone, and potassium hydroxide were of LR grade.

Synthesis of Acrylic Copolymer
The copolymer was synthesized by dissolving maleic anhydride (1 mol) in 100 ml of xylene in a 3-neck flask with inlet for N2 gas, reflux condenser and mechanical stirrer. BMA (exactly 1 mol) containing 1.4 gm of benzoyl peroxide was added drop wise at a constant rate into the flask over the period of 2 hours keeping the temperature constant at 95 °C. The reaction mass was stirred for another 2 hours to complete the reaction. The resulting copolymer was diluted with acetone and precipitated with methanol with constant stirring. Table 1 shows the characteristics of the acrylic copolymer.



Synthesis of Hydroxyethyl Fatty Amide (HEFA)
The oil (0.1 mol) was placed in a multi-necked flask equipped with stirrer, thermometer and condenser, and heated to 150 °C with the diethanolamine (0.34) and zinc oxide (0.002). The temperature was raised to 200 °C and maintained at ± 200 °C until it gave a methanol solubility test. Samples were periodically withdrawn and mixed with two volumes of methanol at room temperature; the disappearance of turbidity showed the completion of the reaction. The formation of hydroxy ethyl fatty amide was further confirmed by a TLC method.7 After reaction completion the product was dissolved in diethyl ether, washed with 15% NaCl solution and dried over anhydrous sodium sulphate. The ethereal solution was filtered and evaporated in a vacuum evaporator to obtain the light-colored hyroxy ethyl fatty amide of dehydrated castor oil. Table 2 shows the physico-chemical properties of hydroxyl ethyl fatty amide of castor oil.

Measurements

Infrared spectra of the synthesized co-polymer were recorded using a Perkin-Elmer 1750 FT-IR spectrophotometer. Molecular weight was determined by GPC (model HPLC 600, RI detector with two ultra styragel columns); polystyrene was used as a standard, and THF as eluent. For DSC analysis, a universal V4.2E TA instruments Q20 differential scanning calorimeter was used. The temperature range was kept as 20-200 °C at the rate of 20 °C/min. The analysis was carried out in an argon atmosphere at the rate of 40 ml/min. The thermal stability of the resin was measured by using a universal V4.2E TA instruments Q50 thermogravimetric analyzer under dynamic scans from 0-600 °C at the rate of 20 °C/min under nitrogen flow at the rate of 30 ml/min. Viscosity of the fatty amide was determined by Brookfield cone and plate 2000 + viscometer, at 25 °C.

Coating Sample Preparation

Coating compositions with varying ratios of acrylic copolymer and HEFA were prepared using xylene/acetone (95/5% v/v) as a solvent. All the compositions were thinned with the above mixture to 50% weight of nonvolatile matter. The sample designations are given in Table 3. Coating films were prepared by applying the various coating formulations on mild steel panels using a bar applicator. Film dry thickness was maintained at 40 ± 5 microns and cured for the evaluation of various mechanical and chemical resistance properties.

Results and Discussion

Spectral Analysis of BMA-MA Copolymer
The IR spectrum of BMA-MA copolymer, shown in Figure 1, shows the presence of an absorption band at 2972 cm-1 due to carboxylic acid of the saturated anhydride. This confirms the inclusion of maleic anhydride in the copolymer. A strong band at 1716 cm-1 may be due to the ester group of the butyl methacrylate.



Spectral Analysis of Hydroxyethyl Fatty Amide (HEFA)
Figure 2 shows the IR spectrum of HEFA. A strong absorption at 720 cm-1 and a weak band at 920 cm-1 can be attributed to (-C-H-) bending arising from poly-methylene groups (-CH2-) groups and (-CH=CH-) groups, respectively, which are present in the fatty amide. A very strong absorption band at 1050 cm-1 is thought to be arising out of (–C-O-) stretching and bending of the primary alcohol. A strong absorption band at 1460 cm-1 can be attributed to (-C-H-) bending and to the presence of tertiary amide. A strong absorption band at 3350-3400 cm-1 may be due to the free (–OH) group.



Molecular Weight
Gel permeation chromatograms are shown in Figure 3. Mn was found to be 8297 and Mw of the resin was found to be 19210.



Thermal Analysis
Figure 4 shows the TGA thermogram of the polyesteramide resin. It is quite obvious that the thermal stability of the resin is quite high as only 10% weight loss is observed up to a temperature of 250 °C. Beyond this temperature a sluggish decomposition takes place and, as a result, about 50% weight loss occurs up to 370 °C and 80% weight loss occurs up to 405 °C.



In Figure 5 an endothermic peak is observed at 155 °C in the DSC thermogram of the resin. The TGA thermogram does not show any significant weight loss at this temperature. The endothermic peak can be attributed to the melting of the resin.


Coating Film Characterization

The various coating formulation panels were cured and tested for different mechanical and chemical resistance properties, as per test methods viz. gloss at 60° (ASTM D 523-99); scratch hardness (ASTM D 5178); pencil hardness (ASTM D 3363-00); and chemical resistance (EN: 438-2:1991). The results are given in Table 4.

Scratch Hardness
Scratch hardness results are shown in Table 4. The comparison of mechanical properties of the films of various compositions reveals that, in general, scratch hardness increases as the amount of curing agent (HEFA) decreases. The scratch hardness property of the film, in general, improves with an increase in the film complexity resulting from a higher degree of crosslink density. The amount of HEFA has a controlling effect in the scratch hardness of all the coating films. The scratch hardness of coating films decreases as the HEFA content increases. This might be due to the presence of a nonpolar fatty acid moiety in HEFA which brings a plasticizing effect to the films.

Cross Hatch Hardness
Cross hatch was measured by using a cross cut adhesion tester. The test was rated good if 5% of squares were removed. All the coating films showed good cross hatch hardness properties because a significant degree of crosslinking has taken place in the coating films.

Gloss
Gloss was measured using a Triglossometer (Sheen). All the coating films had good gloss.

Flexibility
Flexibility was carried out on ¼ inch Mandrel bend tester. Films of all the coatings compositions were flexible enough to pass (Table 4).

Impact Resistance
Impact resistance was measured using an impact tester. The comparison of impact resistance of the films reveals that, in general, coating films having lower HEFA content have poorer impact resistance, indicating the plasticizing effect of the crosslinking agent in the coating films. The presence of the nonpolar fatty acid moiety of the HEFA is thought to improve the film toughness resulting in the high impact resistance.

Chemical Resistance Properties



Conclusion

Acrylic copolymer was synthesized successfully using butyl methacrylate and maleic anhydride. Hydroxy ethyl fatty amide derived from castor oil was also synthesized and used as a crosslinking agent for these acrylic copolymer/resins to get polyesteramide resins. The study shows that the mechanical and chemical resistance properties of the films are dependant on the HEFA content of the compositions; an optimum acrylic copolymer and HEFA i.e., PE-4 ratio, can be selected to obtain the balanced film properties.

. For further information, e-mail sukhenhbti@gmail.com or dahbti@rediffmail.com.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Department of Oil & Paint Technology, Harcourt Butler Technological Institute, Nawabganji, Kanpur, India
Department of Oil & Paint Technology, Harcourt Butler Technological Institute, Nawabganji, Kanpur, India

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • Country home - sofa and table in modern house

    Reactive Acrylic Copolymers for Use in Low-Extractable Coatings

    See More
  • The Effect of HMMM Crosslinker on the Coating Properties of Chemoenzymatically Synthesized Aliphatic Urethane Oil

    See More
  • Effects of Latex Particle Morphology on the Film Formation and Properties of Fluoropolymer-Based Latex Paints

    See More

Related Products

See More Products
  • nanostructuredthinfilms.jpg

    Nanostructured Thin Films and Coatings: Mechanical Properties

  • thin film.jpg

    Thin Film Coatings Properties, Deposition, and Applications

  • nanostructured.jpg

    Nanostructured Thin Films and Coatings: Functional Properties

See More Products

Related Directories

  • Hexion VAD B.V., Versatic Acids and Derivatives Business Unit

    Hexion's Versatic™ acids and derivatives business unit is the global leader in specialty building blocks for coatings. Resins based on VeoVa™ vinyl esters and Cardura™ glycidyl ester lend unique performance properties to architectural, automotive, and industrial coatings. Hexion new application development focuses on supporting our customers’ sustainability goals and on delivering more sustainable solutions.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing