Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

UV-Curable Polyurethane Acrylate Dispersions Compared to 100%-Solids

By Oscar Valdes-Aguilera, Angela Carmack, Marla de Lombard-Watts
April 5, 2007


The use of waterborne UV-polyurethane dispersions (UV PUDs) has been growing in the areas of wood furniture, kitchen cabinets and automotive products. Typically supplied at 30-40% solids, these UV PUDs are used to formulate sprayable coatings that produce low(er) dry coat weights than can be achieved with 100%-solids UV coatings at room temperature.

Performance properties have been determined using model formulations based on UV PUDs and standard oligomers diluted with butyl acetate. Mechanical properties and chemical resistance of UV PUDs are similar or better than those obtained with standard oligomers, with the additional benefit of physical drying that leads to a tack-free film before UV cure while minimizing VOC generation.



Table 1

Introduction

The increased use of waterborne UV-curable coatings is due to improved product performance, ease of handling and application benefits, and an ever-increasing awareness and concern for the environment. Correspondingly, there is an increasing interest in comparing the performance characteristics of waterborne UV-curable resins to those obtained with standard, 100%-solids UV-curable materials.

Although the benefits of high line speed associated with UV curing are reduced when waterborne UV-curable coatings are employed (water evaporation becomes the slow step in the process), use of these materials is increasing due to other characteristics that cannot be easily obtained with standard UV-curable systems. Some of the advantages of waterborne UV-curable coatings include:1,4,6-8

  • the absence of low-molecular-weight monomers, thus reducing the irritability of the formulation and eliminating their detrimental effect on the properties of the cured coating;
  • thickness control without VOC emission, an important feature in spray applications;
  • ease of design of low-gloss coatings, requiring lower levels of matting agents; and
  • physical drying of the coating, allowing handling and light sanding before UV cure.
This study compares the performance properties of coatings based on waterborne UV-curable resins with those obtained using resins employed to formulate 100%-solids UV-curable systems. Four UV-curable polyurethane dispersions (UV PUDs) are compared with one aromatic (ARUA) and two aliphatic urethane acrylates (ALUA) recommended for use in flooring and furniture applications. All five products are manufactured by Cytec.

Table 1 presents the properties of the products. UCECOAT® 7772, 7849 and 7631 are aliphatic PUDs that give a tack-free film after water evaporation and prior to UV cure. Cured films based on UCECOAT 7772 are characterized by high surface hardness as well as stain and chemical resistance; 7849 imparts flexibility while maintaining stain and chemical resistance; and  7631 has been designed for exterior applications and is characterized by superior weatherability combined with good mechanical properties and chemical resistance.

UCECOAT 7177 is characterized by good substrate and pigment wetting properties. Cured coatings based on this oligomer show surface hardness with high stain and chemical resistance. The film produced after water evaporation is not tack-free before UV cure.

EBECRYL® 4827 is an aromatic urethane acrylate that imparts high flexibility. EBECRYL 284 and 4833 are aliphatic urethane acrylates with good scratch and abrasion resistance, and they are commonly used in flooring applications.

 



Experimental Procedures

Coatings prepared for testing contained 34% resin and 2% ADDITOL® HDMAP as a photoinitiator, the balance being water in the case of UV PUDs and butyl acetate for the 100%-solids UV curable resins.

Formulations were applied with a #10 drawdown bar on transparent vinyl, cold roll steel panels, unlacquered opacity charts and wood veneer (maple and oak). Butyl acetate or water was evaporated at 65 ºC for 10 minutes, and the sample was cured with a Fusion brand EPIQ 6000 unit using two H lamps operated at 600 watt/inch. Typical energy density employed was 1 J/cm2. Thickness of the cured coating was 0.3 mil, measured with a Gardco brand Minitest 100N gauge.

Adhesion to the substrates was determined by the cross hatch method using 3M’s 610 Scotch® brand tape,  gloss at 20º and 60º with BYK Gardner’s micro-TRI-gloss meter and color coordinates with a BYK Gardner Color Guide. Pencil hardness was measured on steel panels using Staedler’s Mars 780 pencil set, flexibility with a conical mandrel, and reverse impact resistance with a BYK Gardner brand impact tester using a 2-lb weight.



Abrasion resistance was determined on opacity charts with a Taber brand Abraser using CS-17 wheels and 1000-g weights. The weight loss after 100 cycles is used as a measure of abrasion resistance. Taber scratch resistance was measured on opacity charts with Taber’s 502 Shear Scratch Tester as the applied weight required to break through the surface. Resistance to MEK was determined by rubbing the surface of the cured coating with cheesecloth saturated with solvent and attached to the head of 2-lb ball-peen hammer.

Stain resistance was determined by placing a drop of staining material on the surface of the cured coating, covering with watch glass to prevent evaporation, and allowing to stand for 24 hours prior to inspection (1 hour for mustard). After removing the staining material, the surface was inspected visually. A more quantitative measure was obtained for mustard and coffee by determining the CIE L*a*b* color coordinates with BYK Gardner’s Color Guide spectrophotometer.

Tensile properties were measured on free films with an Instron brand 4467 tester.  Free films were prepared by applying the formulations on polyester films using 5 mil spacers. Butyl acetate and water was evaporated at room temperature for 24 hours, after which the samples were placed at 65 ºC for 48 hours prior to curing and processing.



Figure 2

Results and Discussion

All coatings had excellent adhesion to vinyl, maple and oak and good adhesion to steel and unlacquered opacity charts. Pencil hardness was between 4H and 6H, and all coatings showed good flexibility and impact resistance.

Table 2 shows results for MEK resistance, Taber scratch and abrasion resistance of the cured films. The aromatic urethane acrylate shows the poorest performance properties of the series, whereas MEK and scratch resistance of the UV PUDs are higher than those obtained with the standard aliphatic urethane acrylates.

The lower abrasion resistance observed for the UV PUDs is attributed to lower resiliency of these resins. As Figures 1 and 2 show, the UV PUDs show similar tensile strength to the ALUAs but significantly lower elongation. The result is lower film toughness and reduced abrasion resistance.



Figure 3

Coatings based on UV PUDs produce films with lower gloss than those based on standard UV resins, the differences being more significant at 20º, as seen in Figures 3 and 4. UCECOAT 7772 gives the lowest gloss and requires lower levels of matting agent to obtain a matt coating. No matting agent is required with UCECOAT 7772 to obtain gloss at 20º in the 15-20 range.



Table 3

Table 3 shows the chemical resistance of cured coatings to a variety of staining materials. This qualitative test indicates that UCECOAT 7772 has the highest chemical resistance and the aromatic urethane acrylate-based coating has the lowest. Stain resistance with mustard and coffee has been quantitated by measuring the change in the CIE L*a*b* color coordinates upon exposure. These materials are the strongest staining materials that are employed in the battery of tests required to obtain certification by the KCMA.

Figure 5 shows the change in the CIE b* coordinate and allows a better visualization of the differences in stain resistance between the UV PUDs and standard UV-curable materials. It should be noted that a change of less than 1 unit in the CIE b* coordinate is virtually undetectable by the naked eye.



Figure 4

In review of the comparative data, the selected UV PUDs (UV-curable polyurethane dispersions) evaluated displayed excellent stain resistance qualities and Taber scratch resistance. These properties are in great demand in a variety of markets and offer added value to the end users. Due to their lower total solids, the UV PUDs would also add ease in handling and end-use application over the undiluted 100%-solids UV systems.

The UV PUDs evaluated in this study displayed equal or better performance properties than the selected aliphatic urethanes, especially in the area of stain resistance, and better performance characteristics than the aromatic urethane.

In overall visual appearance, the UV PUDs exhibited lower gloss than the 100%-solid UV systems, especially at 20º. This low-gloss characteristic is an asset for product lines requiring low sheen while minimizing the level of flattening agents.



Figure 5

Conclusions

The UV PUDs evaluated in this work showed similar or better performance properties than the standard UV-curable urethane acrylates. The viscosity of the coating can be adjusted with water, and the thickness of the cured coating can be easily controlled without VOCs or HAPs emission, all of which are important characteristics in spray applications such as for kitchen cabinets.

For more information, visit www.cytec.com.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Oscar Valdes-Aguilera | Cytec Industries, Inc., Smyrna, GA
Angela Carmack | Cytec Industries, Inc., Smyrna, GA
Marla de Lombard-Watts | Cytec Industries, Inc., Smyrna, GA

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Paint and Coating Market Reports
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • Preparation and Properties of UV-Curable Polyurethane Acrylate Resins for Metal Surfaces

    See More
  • pci0717-Sartomer-528575388-900.jpg

    Low-Viscosity Oligomers for 100%-Solids UV-Curable Soft-Touch Coatings

    See More
  • New Alkoxylated Monomer Offers New Benefits Compared to Commodity Monomers

    See More

Related Directories

  • Eagle Specialty Products

    Serving industrial paint and coatings manufacturers since 1959, we specialize in creating advanced color pigment dispersions for water, solvent-based, and 100%-solids applications. We also offer opportunities for customization. As an ISO 9001:2015-certified company, our research and development team is equipped to create custom colorants and even toll manufacture product. Whether it's Conventional, Low-VOC, or Solvent-Free formulation, we can outfit you with the perfect solution.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing