Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Acrylated Performance Products for Floor Coatings With High Scratch and Abrasion Resistance

November 1, 2005
Floor coatings are commonly used to provide aesthetics and increased durability, especially scratch and abrasion resistance. Wood flooring is normally coated with multiple layers, consisting of a sandable filler, intermediate/build coats and a hard topcoat. In many cases the sandable filler is also used as the build coat. Total coating thickness is between 6 to 10 mils, depending on required wear resistance and cost constraints.

UV-curable coatings are increasingly being used to design floor finishes because of the higher productivity and performance properties achieved with these systems. In addition, since they do not contain organic solvents, UV coatings facilitate compliance with stringent environmental regulations.

Requirements for UV-curable floor coatings include low viscosity for ease of handling and application; fast cure speed; and high resistance to water, stains, scratch and abrasion. Sealers and topcoats based on acrylated urethanes, epoxies and polyesters have been used with differing degrees of success.1-5

Urethane and epoxy acrylates are characterized by high viscosity, thus necessitating relatively high concentrations of reactive diluents to formulate coatings suitable for application. Whereas the use of polyester acrylates mitigates this problem, scratch and abrasion resistance is normally inferior to that obtained with acrylated urethanes and epoxies.1,4

Cytec Surface Specialties has introduced two acrylated performance products to formulate coatings for wood flooring. The products have been designed with low viscosity for ease of handling, with performance properties targeted to wood floor requirements, and for compatibility with standard acrylated oligomers. Typical properties of these products and of an acrylated epoxy, acrylated urethane and acrylated polyester are shown in Table I.

The products shown in Table I have been tested as part of model flooring systems consisting of sealer and topcoat based on these acrylated products. The UV-curable system was compared with a conventional floor coating consisting of solvent-based polyurethane sealer and topcoat. In both cases the sealer was used as an intermediate coat.

Experimental
Formulations and Testing

UV-curable formulations used for testing are indicated in Tables 2 and 3. The resin concentration in the topcoat is either 70% or adjusted to give a viscosity not higher than 1,000 cP at 25 ºC.

Viscosity of the UV-curable formulations was measured with a Brookfield DV-II+ viscometer at 25 ºC. Photospeed was determined by the energy density (mJ/cm2) required to produce a tack-free surface when irradiated with a Fusion EPIQ 6000 curing unit using two H lamps operated at 300 watt/inch. The photospeed was measured on coatings applied on opacity charts with a #12 drawdown bar.

Taber abrasion resistance of the cured coating systems was determined using CS-17 wheels, with 1 Kg weight on each wheel, Hoffman scratch resistance with a Gardco tester, and direct impact resistance with a BYK-Gardner impact tester using a 2-lb weight. The end point for Taber abrasion was breakthrough over 10% of the area in contact with the wheels.

UV-cured coatings were conditioned at 23 ºC for at least 24 hours prior to testing. Following the manufacturer's recommendations, the conventional coating system was allowed to stand at room temperature for at least one week after application of the topcoat. Testing was conducted after conditioning for an additional 24 hours at 23 ºC.

A solventborne floor coating system was applied according to the manufacturer's instructions using materials purchased from a major supplier of wood coatings. The sanding sealer was an oil-modified polyurethane supplied at 36% solids. The topcoat was an oil-modified polyurethane varnish supplied at 50% solids. It was recommended by the manufacturer for its excellent hardness and abrasion resistance.

Application

Solventborne coatings were applied by brushing, and dried at room temperature. All applications and drying were conducted inside a hood due to ventilation requirements. Sanding of the sealer and intermediate coat was conducted 24 hours after application. Physical testing was started not earlier than 7 days after application of the topcoat.

Dry coat weights were (after sanding) 98 g/m2 for the sealer, 71 g/m2 for the intermediate coat and 14 g/m2 for the topcoat. These coat weights are recommended by the manufacturer for high-traffic applications.

UV-curable formulations were applied with a Barberan BRB-800 roll coater on oak veneer. The process was as follows:

    _ sanding of the substrate;

    _ application of the sealer, two coats wet-on-wet;

    _ UV curing;

    _ sanding of the sealer;

    _ application of two layers of intermediate coat, with pre-gelling between applications;

    _ application of final layer of intermediate coat;

    _ UV curing;

    _ sanding of intermediate coat;

    _ application of topcoat; and

    _ UV curing.

Coat weights after sanding were 90 g/m2 for the sealer, 75 g/m2 for the intermediate coat and 14 g/m2 for the topcoat.

Results and Discussion

Figure 1 shows the results for Taber abrasion resistance as determined by breakthrough to the substrate, and Figure 2 shows the Hoffman scratch resistance for the three systems that were evaluated. The latter test uses a cylinder at 45 degrees to simulate scratching by sharp edges.

The higher functionality of RAYLOK 1123 oligomer acrylate (see Table I) leads to a coating with significantly higher scratch resistance than both the conventional system and the finish based on EBECRYL 264 aliphatic urethane acrylate. High Taber abrasion resistance is obtained by high coating resiliency, which is achieved by a proper balance between hardness and flexibility. The higher crosslink density makes the UV coatings more rigid than the conventional system, resulting in lower impact resistance, as shown in Figure 3.

RAYLOK 1123 oligomer acrylate can be blended with more flexible oligomers to obtain a topcoat with higher flexibility but with lower scratch and/or abrasion resistance. Alternatively, since the abrasion resistance obtained with the UV coatings is significantly higher, a lower coat weight can be used to obtain the durability of the conventional system. A lower coating thickness results in higher flexibility due to the reduction in stress associated with higher coat build.

Figures 4-6 present the results obtained with the cost-effective topcoats shown in Table 3. In these experiments, the topcoat based on RAYLOK WF 21 oligomer acrylate is applied over the sealer based on RAYLOK WF 21 oligomer acrylate, whereas the topcoats based on EBECRYL 600 epoxy acrylate and EBECRYL 80 polyester acrylate are applied over the sealer based on the acrylated epoxy/polyester combination (see Table 1).

Scratch resistance of these topcoats is similar to that obtained with the conventional solventborne coating, whereas RAYLOK WF 21 oligomer acrylate and EBECRYL 600 epoxy acrylate can be used to formulate UV-curable coatings with significantly higher abrasion resistance. Based on the viscosity of the products used to formulate cost-effective UV-curable topcoats (Table 1), we conclude that the system based on RAYLOK WF 21 oligomer acrylate represents the best compromise between low viscosity, and high scratch and abrasion resistance.

Conclusions

RAYLOK 1123 oligomer acrylate is a suitable product to formulate high-performance coatings for wood flooring applications. A system composed of a topcoat based on RAYLOK WF 21 oligomer acrylate and RAYLOK 1123 oligomer acrylate, with the sealer and buildcoat based on RAYLOK WF 21 oligomer acrylate show superior scratch and abrasion resistance, with values significantly higher than those obtained with a commercial high-abrasion-resistance polyurethane finish. Topcoats based on these performance products show similar or higher abrasion resistance than topcoats based on standard UV-curable oligomers, and also have lower viscosity and are easier to handle.

Acknowledgements

The author gratefully acknowledges the following from Cytec Surface Specialties: Mr. Greg Bryant, formerly Senior Technical Specialist, for his collaboration with the experimental work, and thanks Dr. Jo Ann Arceneaux, TS&D Manager for Radcure-Americas, and Dr. Jonathan Shaw, TS&D Manager for Industrial Coatings/Radcure-Americas for their thorough review of the manuscript.

References

1 Fei, H. RadTech Asia 2003 Conference Proceedings, 443-447.
2 Burak, L. Paint & Coatings Industry, October 2001.
3 Valdes-Aguilera, O. Paint & Coatings Industry, March 2001.
4 Dulany, L. RadTech North America 2000 Conference Proceedings, 103-112.
5 Ross, J. S.; Leininger, L.W.; Sigel, G.A; Tian, D. RadTech North America 2000 Conference Proceedings, 241-250.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • Acrylated Performance Products for Sandable Sealers

    See More
  • A Novel Concept for Improving Scratch and Abrasion Resistance for Automotive Coatings

    See More
  • pci0620-Evonik-1078115724-lead-900.jpg

    Novel Approaches to Improve Scratch and Abrasion Resistance in UV Coatings

    See More

Related Products

See More Products
  • durability.jpg

    Increasing the Durability of Paint and Varnish Coatings in Building Products and Construction 1st Edition

See More Products
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing