Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Join Today
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • PCI News Now
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Global Top 10/ PCI 25
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • COAT-IT! Podcast
    • Videos
    • PCI Store
    • eBooks
    • Sponsor Insights
  • EMAGAZINE
    • eMagazine
    • Archive Issues
    • Editorial Advisory Board
    • CONTACT
    • Advertise
  • JOIN!

A Unique Fungicide for Wood-Filled Plastic

By Dr. William Woods
March 3, 2008
The agrichemical, folpet, is shown to be an effective fungicide for use in a broad range of plastics including wood-filled plastics. Performance is evaluated through a tiered product development program utilizing: 1. Petri dish and environmental chamber accelerated laboratory testing of weathered samples and 2. the exterior exposure of panels or full-scale constructs (e.g., test decks). The action mechanism of folpet, a trichloro-methylthio-adduct, N-(trichloromethylthio)phthalimide, is discussed herein. The folpet active ingredient is additionally compounded into several physical forms that include resin and lubricant-pellet concentrates and granules for ease of processing into plastics and wood-filled plastic composites based on polyolefins, PVC and other resins. Data are presented that demonstrate protection from microbial defacement and deterioration at use-levels of 0.3 – 0.5% and treatment costs of cents per board-foot of composite without significant impact on physical properties. In addition, thermostability data for folpet and flexural properties of the finished wood plastic composite are presented. Air monitoring during extrusion operations shows that folpet-based products are easily handled safely in the work environment. A manufacturing case study is also presented.

The agrichemical, folpet, is shown to be an effective fungicide for use in a broad range of plastics including wood-filled plastics. Performance is evaluated through a tiered product development program utilizing: 1) Petri dish and environmental chamber accelerated laboratory testing of weathered samples and 2) the exterior exposure of panels or full-scale constructs (e.g., test decks). The action mechanism of folpet, a trichloro-methylthio-adduct, N-(trichloromethylthio)phthalimide, is discussed herein. The folpet active ingredient is additionally compounded into several physical forms that include resin and lubricant-pellet concentrates and granules for ease of processing into plastics and wood-filled plastic composites based on polyolefins, PVC and other resins. Data are presented that demonstrate protection from microbial defacement and deterioration at use-levels of 0.3 – 0.5% and treatment costs of cents per board-foot of composite without significant impact on physical properties. In addition, thermostability data for folpet and flexural properties of the finished wood plastic composite are presented. Air monitoring during extrusion operations shows that folpet-based products are easily handled safely in the work environment. A manufacturing case study is also presented.

Introduction

Folpet belongs to the trichloromethylsulfenyl class of fungicides originally discovered to be effective agrichemicals for the protection of crops, particularly soft fruits, from the growth of plant pathogenic fungi. Folpet is commonly used on hops, avocadoes and grapes. The molecular structure is shown in Figure 1.

The folpet mode of action has been investigated primarily from the viewpoint of the plant pathologist.1-3 Investigations have centered on the mechanism(s) involved in the prevention of the growth of microorganisms that are harmful to plants. Many of these same microbes colonize architectural coatings and stains and flexible PVC plastics; subsequently, trichloromethylsulfenyl pesticides, in particular, folpet, have been found effective as industrial biocides for materials protection.

Initial mode-of-action studies led to the discovery that trichloromethylsulfenyl fungicides (such as folpet) are biological alkylating agents that react with thiols producing compounds that indicate that the primary reaction is the transfer of the trichloromethylsulfenyl group to the sulfur atom of a thiol.4,5 This has been demonstrated in vitro as well as in vivo.6,7 It is generally thought that the principal mode of action involves the reaction of the trichloromethylsulfenyl moiety with cell components containing the thiol functionality. Microbial enzymes are denatured and normal cell division is inhibited.8 The possibility that thiophosgene is a transcient intermediate has been proposed.9

The toxicity of folpet might directly or indirectly result from oxidative stress. Induction of antioxidative enzymes has been reported in several studies that show increase in production of reactive oxidative species in cells.10 Folpet is also described as a potent inhibitor of spore germination by affecting cellular processes required for germination or interfering with respiration.11 To date, the mode of action of folpet has not been fully elucidated.

Folpet is effective in organic solvent-based architectural coatings and stains and flexible PVC plastics for the prevention of fungal organism growth and staining by filamentous bacteria. It is active against mildew and wood-rot fungi. The minimum inhibitory concentrations (MICs) presented in Table 1 illustrate the spectrum of activity of folpet. Based on the proven fungicidal activity in plastics and coating formulations and its broad spectrum of antimicrobial activity, folpet was chosen as a candidate for evaluation in the wood plastic composite matrix.



Additionally, iodopropynylbutylcarbamate (IPBC) was chosen as a candidate. The structure is shown in Figure 2.

IPBC is commonly used as a mildewcide in water-based architectural coating films. The principal mode of action is thought to be through the iodine moiety. Oxidation of the sulfhydryl group of the amino acid cysteine results in loss of the ability to connect protein chains by disulfide (-S-S-) bridges, an important factor in the synthesis of proteins.12

The MICs of IPBC are presented in Table 2. Similarly, about 20 other biocides were chosen for screening based on existing in-house expertise, reviews of the literature and known MIC data.

Biological Testing

First Tier
A tiered evaluation program was used to evaluate the candidate biocides. The first tier of the biocide screen was an accelerated laboratory evaluation in wood plastic matrix in the presence of nutrients. The purpose of this evaluation was to demonstrate activity in the matrix and to establish starting-point use-level ranges for higher tier testing. In addition, the thermal stability of each biocide was evaluated in a Brabender Plasticorder at temperatures and dwell times that simulated process conditions typical of industry extrusion operations.



Test plaques (1.5 cm square x 0.5 cm thick) were inoculated with a mixture of fungal spores in accordance with ASTM G 21-96 and scored for fungal defacement. Photographs of typical ASTM G 21-96 inoculated plates are shown in Figure 3.

A photomicrograph of one of the fungal organisms, Aspergillus niger, used in the inoculum is shown in Figure 4. As seen in Table 3, the biocides showing the best responses were folpet, IPBC, chlorothalonil, Bethoguard, DCOIT (dichlorooctylisothiazolinone) and also Zinc Omadine.

Second Tier
Accelerated testing that included simulated weathering and continuous airborne inoculation in a humidity chamber was used to more closely model exterior exposure and further characterize the performance of the candidate biocides. Test panels, about 5 cm wide x 15 cm long x 0.5 cm thick, were placed in an environmental chamber and tested in accordance with ASTM D 3273 and D 3274.



A set of panels were exposed to UV light with condensed water for 100 hours (QUV, ‘A’ bulb) in order to identify those biocides subject to degradation by UV and water leaching at or near the surface of the wood plastic composite specimen in a moist environment.

A photograph of an ASTM D 3273 Environmental Chamber is shown in Figure 5.

Panels removed from a chamber are pictured in Figures 6-8.

The preparation of test samples using a laboratory scale extruder is shown in Figure 9.

The results of this evaluation are presented in Table 4.

The responses of folpet, IPBC, chlorothalonil, Bethoguard and DCOIT were superior to the other biocides evaluated.



Third Tier, Exterior Exposure
Test panels, about 5 cm wide x 15 cm in length and 0.5 cm in thickness, were exposed on test fences at an orientation of south 45 degrees in three mildew prone regions of the United States: New Jersey, Ohio and Southern Florida. The New Jersey and Ohio responses were closely similar and the data from the Piscataway, NJ site are presented in Table 5; folpet, at 0.3% by weight, demonstrated the best performance.

Resistance to defacement was also demonstrated by IPBC and DCOIT.

Figures 10 and 11 show the response of a concentration ladder of folpet and IPBC after about two years of test-fence exposure in New Jersey.

Sodium hypochlorite solution (bleach) was applied to the top of the defaced control panel as a diagnostic indicator test for biological pigmentation.

None of the biocides performed in the heavily stressed Southern Florida Everglades exposure. All failed at the concentrations tested in about six months.



Test deck exposures in New Jersey of standard board show that folpet at levels of about 0.3% offers protection. Results are presented in Table 6. Figure 10 shows the ‘leopard-spot’ mildew failure often observed on the surface of unprotected deck board.

Strength of Materials

Flexural Properties
In order to evaluate the effect, if any, of biocides on the physical properties of a composite, flexural strength was determined in accordance with ASTM D 6109-05, Flexural Properties of Unreinforced and Reinforced Plastic Lumber and Related Products. Modulus of elasticity and modulus of rupture were determined in the presence of lubricants and coupling agents. The results are presented in Table 7.



Folpet does not appear to have a significant effect on flexural properties in high-density polyethylene (HDPE), polypropylene (PP) or polyvinylchloride (PVC) in the presence of lubricant. Initial findings in the presence of coupling agents are similar. The effect of a biocide or any additive on the mechanical strength of a composite should be evaluated before approval.

As part of this study, folpet compounded as pellets in resin compatible with HDPE and PP and in a lubricant concentrate was successfully processed into wood plastic composite deck board at plant scale. Often the pelletized and granular products are preferred forms in extrusion operations.

Manufacturing

Standard 5.25-inch extruded solid deck board has been produced with folpet at levels of 0.3-1.5 weight percent. A photograph of one of these operations is shown in Figure 13. For those wood composite manufacturers that are not familiar with handling pesticides, training regarding the safe handling of pesticides is available from the supplier.

Conclusion

The tiered approach identified those biocides and use-level ranges required for satisfactory performance in the field. Ultimately, exterior exposure is required to determine duration of protection. Biocide content should be regionalized, if possible, to compensate for differences in climatic and biological stress (mildew susceptibility). Folpet is an excellent candidate for use in wood plastic composite for the prevention of surface defacement by mildew and perhaps wood-rot (soil contact tests are in progress). Starting point use-levels of 0.3 – 0.5% are recommended at treatment costs of about 3 to 5 cents per board-foot of standard deck board.

Acknowledgments

Mr. Rick Mann, Kibbechem, Inc., Elkhart, Indiana; Dr. Karen Winkowski, International Specialty Products, Wayne, N.J.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

International Specialty Products, Wayne, NJ.

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • Double exposure of creative chemistry concept on laptop background, research and development concept

    Inside the AI Shift in Coatings

    Industry leaders share real-world examples of how AI is...
    Industrial Coatings
    By: PCI Editorial Staff
  • Global Top 10 and PCI Logo

    2026 Global Top 10: Top Paint and Coatings Companies

    See how the world’s largest paint and coatings companies...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • The 2026 PCI 25

    2026 PCI 25: Top Paint and Coatings Companies

    See how North America's largest paint and coatings...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • Join Paint & Coatings Industry
  • Manage My Preferences
  • Customer Service

More Videos

Popular Stories

Breaking News

H.B. Fuller to Close Seven Sites in Supply-Chain Overhaul

AkzoNobel Axalta

EU Clears $25B Akzo-Axalta Merger with One Big Condition

A robotic hand points at a glowing compliance concept surrounded by various icons representing laws, regulations, governance, and standards in a digital workspace

Powder Coater’s $1.64M OSHA Case Follows Earlier Citations

Events

December 2, 2026

Self-Activated Binder Technology: A New Path to Tin-Free Polyurethane Coatings

Through examples from protective and general industrial coating applications, attendees will learn how these innovative technologies can help maintain, and in some cases improve, coating performance while supporting safer, more sustainable formulations that align with evolving regulatory expectations

December 10, 2026

PC Academy: Waterborne Polymers and Film Formation

The trend towards waterborne polymers in the paint and coatings industry is clear; highlighting their environmentally friendly nature, regulatory considerations, growing market demand, and meeting sustainability goals.

View All Submit An Event

Products

Powder Coatings - Foundation for the Novice Formulator (ebook)

Powder Coatings - Foundation for the Novice Formulator (ebook)

See More Products
PCI news now promo ad

Related Articles

  • A Unique Color Mixing System for Colored Wood Stains and Varnishes

    See More
  • valspar

    Valspar helps Writers Theater achieve a unique architectural look

    See More
  • Intense Red Effect Pigment with a Unique Sparkle.jpg

    Intense Red Effect Pigment with a Unique Sparkle

    See More

Events

View AllSubmit An Event
  • September 16, 2026

    Generative AI: A Hammer Looking for a Nail? Or a Powerful Tool in the Toolbox?

    On Demand Generative AI, Machine Learning, and Statistical Modeling aren't interchangeable — they solve different problems at different stages of development. Use the wrong one and you're led astray. Use the right one and you compress months of R&D into weeks.
View AllSubmit An Event

Related Directories

  • ProSys Fill LLC

    ProSys Fill manufactures high-performance filling and packaging equipment for paints, coatings, sealants, and other demanding materials. Our American-made systems are engineered to handle challenging viscosities while delivering reliable, accurate filling and efficient changeovers. From standalone fillers to complete packaging lines, ProSys helps manufacturers reduce downtime, minimize waste, and keep production moving.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Manufacturing Division
  • JOIN TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing