Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

A Solid Epoxy Resin Emulsion for Acrylic-Epoxy Coatings

By Lorenzo N. Petway
April 1, 2009
A new waterborne solid epoxy resin emulsion (Araldite® PZ 3921) was designed to meet the need for improved durability, resistance and aesthetics when formulated into a two-component acrylic-epoxy coating.

Waterborne, two-component acrylic-epoxy coatings have become increasingly popular in the areas of high-performance architectural and light industrial maintenance. These coatings offer improved performance properties compared to typical waterborne acrylic emulsion-based coatings commonly used for these applications. Waterborne two-component acrylic-epoxy coatings offer the benefits of improved durability, improved resistance to food stains, household and industrial cleaners, low odor, and low VOC content. These coatings also offer the applicator the ideal properties of long pot life (typically more than 24 hours), fast dry times and easy clean up with soap and water. These versatile coatings are suitable for use on many common substrates, such as drywall, concrete block, galvanized steel, ferrous metals, masonry, plaster, stucco and wood.

The ideal application areas for these paints include many institutions and facilities such as: schools and universities, churches, hospitals, extended care facilities and department stores.

In most architectural applications the appearance of the coating is of utmost importance. The coating must be able to withstand frequent, and often vigorous, cleaning by the institutions’ maintenance staff, reducing the need to repaint. Therefore, durability and resistance to marring, stains and cleaning solutions and good aesthetics is critical.

Current Technology

Today, the majority of waterborne two-component acrylic-epoxy coatings are formulated using a carboxyl-functional acrylic latex resin with a waterborne “1-type” solid epoxy resin emulsion as the binder. It is also possible to use standard liquid epoxy resin emulsions in combination with the acrylic resin. Coatings that use liquid epoxy resins typically have high gloss and shorter pot life.

The epoxy and acrylic resin react, albeit slowly, to provide the coating with the aforementioned properties. The ultimate properties of acrylic-epoxy coatings are reached over a period of 2-4 weeks of cure under ambient conditions.

A New Solid Epoxy Resin Emulsion



A two-component acrylic-epoxy paint was developed to demonstrate the benefits of Araldite® PZ 3921 when compared to the standard emulsion in the same formulation. Paint formulation properties, prepared from each emulsion, are listed in Table 2.

The paint formulations were adjusted to have the same acrylic:epoxy ratio, mixing ratio and solids content to facilitate the performance comparison.

Formulated Paint Testing

The formulated paints were tested to determine their performance properties using standardized test methods appropriate for the intended application.

Testing Protocol
An induction time of 1 hour at 23 °C was given to both systems, which were then applied onto cold rolled steel panels (Q-Panel® S-48 SAE 1008/1010 panels; 0.032 in., ground finish) with a 5-mil drawdown bar. The paint films were cured at 23 °C and 50% relative humidity for 7 days before testing, unless otherwise specified. The test protocol used to evaluate the performance of the coatings is listed in Table 3.



Test Results
The results of the testing are shown in Table 4. The acrylic-epoxy paint based on Araldite® PZ 3921 performed similarly to the coating based on the standard emulsion in most areas including dry times, gloss, adhesion, flexibility and abrasion resistance. However, the Araldite® PZ 3921-based paint did show significant improvements over the paint formulated with the standard emulsion in some key areas.

An important and substantial improvement was found in the scrub resistance. The Araldite® PZ 3921 system exceeded the performance of the control by nearly 2,600 cycles (79% increase) in scrub resistance testing showing the paints’ outstanding durability. A large improvement in impact resistance was also observed. Such an increase is very important for application on items fabricated from thin metal substrates, such as office furniture. The excellent inter-coat adhesion of the Araldite® PZ 3921 coating allows the applicator to apply up to several coats of the paint in an eight-hour period, resulting in increased productivity. The coating based on the standard emulsion does seem to have a longer recoat window, however.



The Araldite® PZ 3921 paint possesses a pot life in excess of 31 hours at 23 °C. The paint shows consistent performance in terms of mixed viscosity and gloss and adhesion of the cured film over this induction period as shown in Figure 1. The testing was discontinued after 31 hours. An extended pot life determination was not performed with the standard emulsion paint.

Conclusion

Waterborne, two-component acrylic-epoxy coatings offer better performance properties than acrylic latex paints, lending to their use as high-performance architectural and light industrial coatings. Among the benefits of these paints are better durability, abrasion resistance, stain and chemical resistance, and water resistance.

A new epoxy resin emulsion Araldite® PZ 3921 was developed to improve the performance of these paints, specifically by making them even more durable. The Araldite® PZ 3921 emulsion increased the scrub resistance by 2,600 cycles, a 79% increase over the standard emulsion used for these applications. This feature provides longer lasting and, thus, more economical paints for use in high traffic areas that require frequent cleaning.

The paints based on Araldite® PZ 3921 also proved to be more impact resistant, a favorable feature for light-duty coatings for metal, such as those for office furniture. In the face of tightening VOC limits, Araldite® PZ 3921 also offers the potential for lower VOC content coatings due to its lower solvent content compared to the standard epoxy emulsion.

For more information, visit www.huntsman.com.
All information contained herein is provided "as is" without any warranties, express or implied, and under no circumstances shall the authors or Huntsman be liable for any damages of any nature whatsoever resulting from the use or reliance upon such information. Nothing contained in this publication should be construed as a license under any intellectual property right of any entity, or as a suggestion, recommendation or authorization to take any action that would infringe any patent. The term "Huntsman" is used herein for convenience only, and refers to Huntsman Corporation, its direct and indirect affiliates, and their employees, officers, and directors.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Scientist Sr., Coatings and Construction, Huntsman Advanced Materials, The Woodlands, TX

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Paint and Coating Market Reports
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • New Curing Agents for Dimensionally Stable, Aqueous Epoxy Resin Coatings

    See More
  • Novel Waterborne Epoxy Resin Technology for Zero-VOC 2K Coatings

    See More
  • BASF Offers Epoxy Resin Systems For Wind Turbine Blades

    See More

Related Products

See More Products
  • marketsandmarketslogo.jpg

    Protective Coatings Market by Resin Type...

  • Hansen Solubility Parameters – A Scientific Approach for Coating Formulators (Virtual Course - 8/20/26)

  • Principles and Applications of Emulsion Polymerization

See More Products

Related Directories

  • IGM Resins

    IGM Resins provides a broad range of photoinitiators, oligomers (epoxy, polyester and urethane), acrylate monomers and additives to address every formulating need.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing