Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

A New Generation of Sparkling Effect Pigments

October 1, 2004
The pigment industry offers an extensive range of classical and effect pigments. Effect pigments are platelets with diameters mostly in between 5 and 50 microns. They reflect incident light and cause angle-dependant lightness effects. Additionally, the incoming light can be modified through absorption and/or interference effects. The high number of possible combinations of layers of different materials, and the variation of layer thicknesses make the world of effect pigments rather complex.

A classification according to coloristic properties provides an overview. Effect pigments can be transparent, semitransparent or opaque in nature. The coloristic impression of effect pigments can be black, silver, colored or goniochromatic. In a simple picture, the existing pigments can be arranged according to these properties (Figure 1).

Along the horizontal axis the effect pigment world is classified according to transparency: opaque groups are 1, 2, 5 and 8; semitransparent are pigments in groups 3, 6 and 9; and transparent pigments are in groups 4, 7 and 10.

Along the vertical axis the classification criterion is the optical impression of the effect pigments. For example, the second row contains silver pigments based on opaque (2), semitransparent (3) or transparent (4) flakes. Aluminum flakes are the examples for opaque silver pigments (2), titanium oxide-coated micas represent transparent silver pigments (4), while micas coated with grey to black oxides are semitransparent (3).

Goniochromatic effect pigments show different colors at different viewing angles. Here as well, opaque types (8), semitransparent (9) or transparent grades (10) exist. These are described elsewhere in numerous publications1 and are not an item of discussion in this paper.

This paper concerns colored opaque effect pigments (5), which are of high relevance in the field of effect coatings. Their unique combination of colored gloss and hiding power is highly appreciated in automotive finishes. Iron oxide-coated aluminum flakes with golden and orange hues are examples for this important group. To date, the iron oxide-coated aluminum platelets are based on aluminum flakes of the cornflake type. Effect coatings based on such pigments show a smooth appearance2 (Figure 2).

During recent years, sparkling effects have strongly increased. Mainly semitransparent or transparent pigments based on metal oxide-coated aluminum oxide or micas have been used to create angle-dependant sparkling effects in directed light.3

This paper introduces a new generation of sparkling effect pigments. They belong to the opaque colored effect pigment type (5). They offer vivid, sparkling, new shades and surprising new possibilities in design.

Iron Oxide-Coated Aluminum Flakes

The optical impression of iron oxide-coated aluminum flakes is determined by a combination of reflection, absorption and interference of light. Incoming light is split - a part is reflected at the surface, the other part of light enters the iron oxide layer and is totally reflected at the aluminum surface. As a result, reflected light is modified by absorption and interference phenomena (Figure 3).

With increasing thickness, the interference color of iron oxide-coated aluminum pigments show golden, orange or red shades. Due to the selective absorption of Fe2O3, blue interference colors of thin iron oxide films are dull.

Iron oxide-coated aluminum flakes are manufactured in a chemical vapor deposition process. Vapors of a precursor [Fe(CO)5] are oxidized in the presence of aluminum powder. During the oxidation Fe2O3 is formed as a thin film on the Al-surface.2

A New Generation of Sparkling Effect Pigments

To date, aluminum of the cornflake type has been used as starting material for the iron oxide-coated aluminum. Those pigments show excellent hiding, high chroma and medium lightness. Due to the thin flakes, coatings were of smooth appearance. The new generation is based on silver dollar aluminum, which is brighter and shows more sparkling effect than the cornflake grades. (Figure 4)

New Gold ED 7866

An iron oxide layer of 20 nm creates a strong golden interference color on the surface of the silver dollar substrates. Compared to cornflake-based grades, the silver dollar-based ED 7866 shows higher chroma and a more pronounced lightness flop. Figure 5 illustrates the coloristic differences between the two grades in full shade.

In paint design, the pigments can be used to create a vivid sparkling effect. Compared to golden sparkling pigments like iron oxide-coated micas or titanium oxide-coated alumina flakes, hiding is significantly better.

New Red ED 7621

An iron oxide coating of 120 nm on the surface of silver dollar flakes is creating a brilliant red effect shade. The red interference color and the selective absorption of iron oxide in the blue range yields highest chroma values (Figure 6). The comparison with red effect pigments representing the state of the art shows the tremendous advantages in coloristic properties: higher chroma, higher lightness, better hiding (Figure 7).

In further tests, a formulation with Red ED 7621, Pigment Red 179 and Pigment Black 6 has been sprayed out. Compared to red micas or red, iron oxide-coated alumina flakes the composition with red iron oxide-coated silver dollars shows extreme high chroma and lightness (Figure 8).

New Sparkling Pigments Based on Platelike Iron Oxide

Under normal aqueous precipitation conditions, iron oxide red crystallizes in the form of octahedrons. By the use of more unusual conditions, like hydrothermal synthesis methods, other crystal shapes are possible.

In the past, platelike iron oxide has been synthesized starting with an alkaline aqueous suspension of FeOOH. The suspension is heated in a hydrothermal reactor. Due to the addition of small amounts of aluminum and manganese salts and hydrothermal conditions (high pressure, high temperature), the needle-like FeOOH crystals are transformed to plate-like Fe2O3-pigments (Figure 9).

The thickness of the resulting flakes can be varied from ~ 100 to roughly 1500 nm. A lower amount of aluminum oxide increases the thickness of the hydrothermal synthesized iron oxide flakes. The resulting thicker flakes, with thicknesses of more than 500 nm, show interesting sparkling effects in sunlight (Figure 10).

In Figure 10, the microscopic pictures on the top are made with bright field illumination mode. The thinner flakes show weak interference colors, because thicknesses are in the range of around 200 nm. A lower ratio of Al:Mn during the hydrothermal step increases the thickness: no more interference colors are visible. The medium flake diameter is nearly unchanged. The pictures on the bottom have been made by using the dark field illumination mode of the microscope. The sparkling flakes are thicker and opaque, while the less sparkling flakes are semitransparent and copper colored.

Styling Possibilities With Sparkling Iron Oxides

In combination with carbon black, the thicker iron oxide flakes show neutral and vivid sparkling. As the color of the flakes is a neutral grey, they can be used in all shade areas. In diffuse illumination no effect is visible; in directed light an eye catching, "starry sky effect" is possible.

Summary

New sparkling effect pigments are possible through iron oxide coating of aluminum flakes of the silver dollar type. The resulting golden, orange or red colored silver dollars show high chroma and hiding power in combination with sparkling effects.

Through hydrothermal treatment of suspensions of needle-like iron oxides, sparkling iron oxides have been synthesized. The sparkling iron oxide flakes are interesting for dark shades with "starry sky effect".

For more information, contact the authors at BASF AG, 67056 Ludwigshafen Germany.

References

1 Schmid, R.; Mronga, N.; Radtke, V., and Seeger, O. Luster Pigments with Color Variable Properties. Eur. Ctgs. J. 7-8,1997.

2 Mronga, N.; Schmid, R. New Pigments by Chemical Vapor Deposition. The Future of the Color Pigments Industry - Conference of the Color Pigment Manufacturers Association, Washington D.C., April 1998.

3 Maile, F.J.; Reynders, P.; Substrates for Pearlescent Pigments. Eur. Ctgs. J. 4, 2003.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Paint and Coating Market Reports
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • A New Generation of Indanthrone Blue Pigments

    A New Generation of Indanthrone Blue Pigments

    See More
  • Potential for a New Generation of Solar-Reflective Coatings

    See More
  • pci1220-Bitrez-627864824-Lead-900.jpg

    A New Generation of REACH-Compliant Ketamine Epoxy Curing Agents

    See More

Related Products

See More Products
  • pci january 2020

    PCI January 2020 Issue

  • pci october cover

    PCI October 2019 Issue

See More Products

Related Directories

  • Schlenk Metallic Pigments

    SCHLENK supplies state-of-the-art metallic pigments, including solvent and waterborne aluminum and gold bronze pigments for all coatings and paint applications. In addition, we supply unique special effects like our Zenexo® ultra-thin colored aluminums that offer unmatched durable gold and orange effects. Our very broad Decomet® vacuum metallized pigment line allows formulators to achieve very smooth metal and chrome-like effects. SCHLENK products are available globally.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing