Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Energy-Curable Lithographic Inks

By Rosalyn Waldo
June 21, 2007
The Influence of Acrylated Oligomer Properties on Ink Misting

Table 1


Ink misting remains a challenge with energy-curable lithographic inks. Approaches to control misting or ink-fly include using inert fillers or other rheology modifiers to build ink body. While effective in reducing misting, these methods often adversely affect other ink properties.

In conventional inks, resin properties such as viscosity, internal cohesiveness and viscoelasticity greatly influence their misting tendencies. Is the same true of acrylated oligomers? In this paper we explore the relationship between oligomer properties such as viscoelasticity and tack, and the oligomer’s tendency to exhibit misting.

Table 2

Experimental Procedures

Tack, an ink term, can be defined as the cohesiveness of an ink film. This cohesiveness is responsible for the ink film’s resistance to splitting. The same definition can be applied to an acrylated oligomer. Every oligomer will have some degree of internal cohesiveness, or tack, and the oligomer’s chemical classification has a strong impact on its viscosity and tack (Table 1). Low-molecular-weight, high-viscosity epoxy acrylates have high oligomer tacks. In comparison, polyester acrylates have higher molecular weights and lower viscosities. Their oligomer tacks are relatively low.

As expected, the rheological properties of these oligomer types are also different. For confirmation, oscillation sweeps of selected epoxy and polyester acrylates were performed on a TA International AR 2000 rheometer. Results indicated that both oligomer types have low storage modulus (G’), but very different loss modulus; the epoxy acrylates had high G’ while the polyester acrylates were much lower. This difference in the loss modulus is supported by the differences in the apparent viscosities of epoxy and polyester acrylates.

The viscoelastic nature of these oligomers can be evaluated by comparing the ratio of their loss storage modulus or tan delta. It is accepted that a tan delta greater than one indicates a viscous nature and a tan delta less than one indicates elasticity.



Table 3

The high strain region of the sweep was the focus of our evaluation. At the deflection point, the point of initial response to increasing strain, the loss modulus of the epoxy acrylates exceeded the storage modulus, giving a positive tan delta. These acrylates are viscous and not elastic. For most of the polyester acrylates tested, the tan delta at this point was negative; these oligomers had a more elastic nature.

Oligomer elasticity will allow the bonds to stretch and exhibit less rupturing under strain. This should result in lower oligomer misting. Table 2 shows oligomer tack, tan delta at the deflection point, and misting off the inkometer at 400 RPM. The more elastic polyester acrylate exhibits low oligomer misting but so does the more viscous epoxy acrylate. The lack of oligomer misting with the epoxy acrylates is a direct result of high internal cohesiveness. The strength of the intramolecular bonding causes this strong resistance to film splitting or misting. A notable exception to low misting with the polyester acrylates was the higher viscosity fatty acid modified oligomer. Under our test conditions, this particular polyester acrylate was determined to be viscous, not elastic. The higher oligomer misting can be attributed to  its lower internal cohesiveness and lack of elasticity.

For the next phase of our evaluations, inks were prepared using the formulation in Table 3. The test oligomer was used in both the pigment dispersions and letdown portions of the ink. Ink tack testing was completed in accordance with ASTM test method, D 4361. The misting tendencies were identified by calculating the total color difference, DE, between unexposed charts and those placed beneath the inkometer rollers during misting testing.



Table 4

Table 4 shows a comparison of oligomer and ink properties. As seen with the oligomer tacks and misting, the influence of the strong internal bonding found in the epoxy acrylates resulted in high ink tack and low ink misting. While advantageous from a misting perspective, this strong bonding has some drawbacks. Higher ink tacks can be problematic for high-speed printing or printing on some porous stock. These high-tack inks typically exhibit little ink flow and can experience transfer problems on press. Adding monomer or other low-molecular-weight diluents to reduce ink tack usually results in significantly increasing the misting.

Compared to epoxy acrylates, polyester acrylates have less hydrogen bonding. This leads to lower oligomer viscosity and tack. Polyester acrylates exhibit elasticity – there is less rupturing under strain. The inks made with polyester acrylates have suitably low ink tacks and low ink misting.

Conclusions

The rheological properties of acrylated oligomers have a major influence on ink properties. While viscous oligomers can be used to achieve lower misting, they will also have higher ink tacks, which could impact their usability and printability. The use of elastic oligomers allows the formulator increased latitude in developing inks with low ink tacks and low ink misting.

Acknowledgements

The author wishes to thank Ms. April Stevens, Chemical Technician, Graphics-RADCURE™ and Mr. Gordon Meyer, Scientist II, Industrial Coatings-RADCURE™, for their assistance offered on this study. For further information see www.cytec.com.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Rosalyn Waldo, Research Associate, TS&D Graphics-RADCURE | Cytec, Smyrna, GA

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • UV Curable Inks Market Expected to Reach $3.5 Billion by 2020

    See More
  • pci0518-Allnex-478100980-900.jpg

    Use of Amino Acrylates to Reduce Photoinitiator Concentration or Increase Cure Speed in UV LED-Curable OPVs and Flexo Inks

    See More
  • UV-Curable Inks

    See More
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing