Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Low Viscosity, Fast Curing Epoxy Acrylate Oligomers

September 27, 2000
Conventional epoxy acrylates based on diglycidyl ether bisphenol A are the most frequently used oligomers in the ultraviolet light (UV) curing industry because they are hard, fast curing, and offer excellent abrasion and chemical resistance. Unfortunately, the inherent hardness of these oligomers has several negative side effects, including yellowing over time, high viscosities and poor adhesion.

Recently, a major specialty chemical manufacturer conducted testing to develop new epoxy acrylate oligomers that offer all of the traditional advantages of using an epoxy acrylate without yellowing. In the testing, a diacrylate low viscosity oligomer (CN-132) and a triacrylate low viscosity oligomer (CN-133) were compared to a difunctional bisphenol A-based epoxy acrylate (CN-120). A variety of performance properties were evaluated to determine the utility of these oligomers as replacements for typical epoxy acrylates in wood coating applications.

Cure Methods

Researchers evaluated CN-132, CN-133 and CN-120 without using monomers as diluents. They were cured using 4% of a highly reactive, non-yellowing photoinitiator for the photopolymerization of UV-curable systems. This photoinitiator was composed of a liquid oligomeric alpha hydroxy ketone and 2-hydroxy-2-methyl-1-phenyl propane mixture.

Researchers used an aluminum chromate Q-panel substrate, and drew the films down using a number 40 wire wound rod, which ultimately yielded films with a thickness of 2 mils. The films were cured at 50 feet per minute using a 300-watt per inch mercury lamp.

Performance Testing

Performance properties evaluated include: pencil hardness, chemical resistance, maximum rate of cure speed, adhesion, abrasion resistance and Hoffman scratch.

Figure 1/ Pencil Hardness

Pencil Hardness

Pencil hardness is determined using a calibrated set of drawing leads that range from 6B (the softest) to 6H (the hardest). The first pencil that scratches the surface is reported as the coating’s hardness. This is specified as ASTM D 3363.

The results, shown in Figure 1, indicate that CN-133 performs as well as CN-120. CN-132 also performs well but is not as hard. However, the actual difference in pencil hardness is insignificant.

Figure 2/ MEK Resistance

Chemical Resistance

Chemical resistance testing using methyl ethyl ketone (MEK) is an indication of the degree of crosslinking associated with a given film; the higher the MEK resistance the better the cure. It was tested as outlined in Appendix 8 of Radiation Curing Test Methods. Figure 2 shows that testing was ended at 200 MEK double rub cycles, the maximum number of rubs performed in this test. The data reveals that CN-132, CN-133 and CN-120 have excellent MEK resistance and reached the maximum resistance.

Figure 3/ Surface Cure Speed

Maximum Rate of Cure Speed

The maximum rate of surface cure was determined using a 300-watt per inch Hg bulb. The fastest conveyor line speed at which a tack free cure is still attained is recorded in Figure 3.

The findings represented in Figure 3 indicate that CN-132 and CN-133 outperform CN-120. The difference in cure between CN-132 and CN-133 is significant, but the difference between these two oligomers and CN-120 is even more significant.

Figure 4/ 610 Tape Adhesion

Adhesion

Adhesion is a measure of the force required to remove the coating from the substrate. Tests were conducted in accordance with ASTM D 3359 using 610 tape.

Figure 4 illustrates that CN-132 and CN-133 outperform CN-120 again. Adding adhesion promoting monomers or low functionality monomers can enhance adhesion even more.

Figure 5/ Taber Abrasion Resistance

Abrasion Resistance

Abrasion resistance is one of the most complex properties to achieve, as it is both a surface and sub-surface property. Thus, abrasion resistance can involve different mechanisms that may be interrelated.

Taber abrasion relates to the ability of a coating to resist abrasive wheels. All panels were tested in accordance with ASTM 4060-84. Taber abrasion resistance was tested under varying loads using a CS-17 wheel with a 1,000-gram load for 500 cycle intervals. Milligrams of weight loss per 500 cycles are recorded.

As Figure 5 illustrates, CN-132 failed with the 2,000-gram load. CN-133 showed improvement in abrasion resistance when compared to CN-120 for all of the loading levels.

Figure 6/ Hoffman Scratch Resistance

Hoffman Scratch Resistance

Hoffman scratch resistance is measured by placing a load on a stylus. The weight of the load required to mar and scratch the surface was measured.

As illustrated in Figure 6, CN-132 and CN-133 significantly outperform CN-120 in mar resistance. In addition, the triacrylate oligomer exhibits slightly better scratch resistance than the conventional epoxy acrylate oligomer.

Conclusion

The newly developed, low viscosity, non-yellowing CN-132 and CN-133 oligomers can replace conventional epoxy acrylates in many applications, including wood coatings. These products outperform bisphenol A-based epoxy acrylates (CN-120) in several key performance properties. CN-133 has equivalent pencil hardness and chemical resistance with superior surface cure speed, adhesion, abrasion resistance, and scratch resistance. CN-132 also offers non-yellowing characteristics with extremely low viscosity, superior surface cure speed, and adhesion in comparison to CN-120.

For more information on oligomers, contact Sartomer Co., Oaklands Corporate Center, 502 Thomas Jones Way, Exton, PA 19341; phone 610/363.4199; fax 610/594.0252; e-mail burak@sartomer.com; visit www.sartomer.com.

Links

  • Sartomer Co.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • New Radiation-Curable Polyester Acrylate Oligomers

    See More
  • Dymax Presents New Developments in Acrylate Oligomers for 3D Printing

    See More
  • Advances in the Chemistry of Melamine Acrylate Oligomers

    See More

Related Products

See More Products
  • pci january 2020

    PCI January 2020 Issue

See More Products

Related Directories

  • Miwon North America Inc.

    Miwon North America products: Miramer Acrylate Oligomers (Epoxy, Urethane, Polyester, and Specialty Oligomers), Miramer Arylate and Methacrylate monomers, Benzoin (powder coatings), Sucrose Benzoate (SB).
  • Kowa American Corp.

    Offers the widest selection of specialty and UV-curable monomers, including Acrylates, Methacrylates, Acrylamides, vinyl ethers, Thiol-ene and cycloaliphatic expoxides. Organic microspheres for matting agents/abrasion resistance. VOC-exempt solvents DMC and PCBTF. Low viscosity & waterborne HDI specialty resins. Low-MW acrylic polymers with silyl, hydroxy or carboxy functionalities used as reactive liquid polymers.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing