Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

New Additive to Enhance Surface Cleanability

June 5, 2003


Figure 1 / Water Droplet "Collecting" Dirt (Hydrophilic) on a Lotus Leaf
The term "Lotus-Effect[R]" represents the replication of the self-cleaning properties of lotus leaves on man-made surfaces. It has gained recent attention in literature as well as in some end-use applications. The effect is based on a very hydrophobic surface that is also micro-structured. This article discusses the potential for obtaining similar effects in coatings using additives without the need for micro-structured surfaces. This approach permits the creation of transparent and high-gloss coatings that are significantly easier to keep clean than conventional painted surfaces.

A new hydroxy- (OH) functional silicone modified acrylate additive can enhance the surface-cleaning properties (cleanability) of coatings. Crosslinkable by way of OH-groups, BYK-Silclean[R] 3700 provides long-lasting significant improvements in cleanability so that adhering dust and dirt particles as well as graffiti can be removed much easier compared to "normal" surfaces.

Figure 2 / Even Hydrophobic Materials, Like This Red Dye, Can Be Washed from the Surface By Water

Lotus-Effect

The phenomenon of the water repellency of plant leaf surfaces has been known for many years. The correlation of water repellency and self-cleaning properties of such surfaces has only recently been investigated in detail1: the adhesion of contaminating particles ("dirt") is greatly reduced, and water droplets rolling across the surface can easily pick up the contaminating particles to leave behind a cleaned surface (see Figures 1-2).

Figure 3 / Micro-Structure of Lotus Leaf Surface
The large leaves of the lotus plant show this effect in dramatic fashion, thus the term "Lotus-Effect" was coined. However, this effect can also be observed with other plant leaves.

The Lotus-Effect itself is based on surface roughness caused by microstructures (see Figure 3) in combination with a highly hydrophobic surface. The combination of both properties reduces the contact area between solid particulates or droplets of liquid on the leaf's surface drastically; liquids such as water, exhibit very high contact angles (see Figure 4).

Figure 4 / High Contact Angle of Water Droplet on a Lotus Leaf
Due to the very small area of surface contact, the adhesion of solid particulates and water is significantly reduced, resulting in the observed self-cleaning effect. The mechanism of this combination of micro-structure and hydrophobicity is shown in Figure 5.

Once the principles of this effect were understood, it was possible to replicate it artificially on surfaces such as facades, roofs and coatings. The biological system was used as a model to improve the properties of these man-made surfaces. For demonstration purposes, Figure 6 shows a plastic spoon that is partially coated with a micro-structured, hydrophobic coating; the self-cleaning properties are clearly visible.

A consequence of the necessary micro-structure is that high-gloss surfaces are not possible. Surface structure always leads increased diffusion and reduced reflection of light, resulting in a flatted or low-gloss appearance.

Figure 5a / Conventional Surface; Water Droplet Running Across the Surface Will not Remove Dirt Particles.

Lotus-Effect in Coatings

To transfer the Lotus-Effect into coatings, it is necessary to create a hydrophobic surface with very low surface tension, along with the appropriate micro-structure. Additives can contribute to the Lotus-Effect by increasing hydrophobicity and reducing surface tensions. Such additives will not create the necessary micro-structure; the structure must be introduced by other means (e.g., high amount of suitable extender pigments, etching, stamping).

This article introduces a new surface additive that can be used for Lotus-Effect coatings. In the absence of a micro-structure, the true Lotus-Effect is not created but something that comes very close is: the resulting surface does not have self-cleaning properties but it is much easier to clean than conventional surfaces. The absence of the surface micro-structure allows high-gloss and transparent coatings to be formulated.

Figure 5b / Highly Hydrophobic Surface with Micro-Structure; Water Droplets are Able to Pick Up the Dirt Particles and Remove Them from the Surface
Contact angle measurements of water droplets show that with the additive alone, a very high angle of about 125 deg can be achieved, in combination with the micro-structure the contact angle can be increased to approximately 160 deg (compared to 40 deg for conventional surfaces such as glass).

Figure 6 / A Plastic Spoon Partially Coated with a Micro-Structured, Hydrophobic Coating (Right Side). After dipping in honey, the self-cleaning property due to the Lotus- Effect is clearly visible.

Introduction of a New Additive

An easily cleaned surface is an important target of new developments not only in architectural coatings but also general industrial coatings (e.g., coatings for household appliances), wood coatings (e.g., kitchen cabinets), plastic coatings (coatings for consumer electronics) and marine paints. Fluorinated resins are well known not only for superior durability but also for their excellent dirt-releasing properties. A specialty application coating in the architectural market uses a very hydrophylic surface that is easily cleaned by rain. This easy surface-cleaning property, or cleanability, is typically a function of the specific binders selected to form the film. However, good cleanability can also be obtained with "conventional" binders when they are modified with certain additives. Among those additives, crosslinkable silicone containing polymers provide a unique set of properties.

Table 1
Silicone additives are known for their beneficial effects in coatings. Polyether or polyester-modified silicones not only provide good surface flow and substrate wetting, but also improvement of surface slip and mar resistance. However, the improvement of surface slip and mar resistance is limited because the silicone on the coating surface can be washed or wiped off. OH-functional polyester or polyether-modified silicones can provide longer lasting surface slip properties, but improvement of surface cleanability is not completely satisfactory.

Table 2
A new, special silicone-modified OH-functional acrylate additive has been developed; the structure is optimized to meet the main objective of providing excellent surface cleanability. This new development not only provides easily cleaned surfaces in OH-crosslinking binders, but also improves surface flow, substrate wetting, and slip and mar resistance. Table 1 shows the properties of this new additive.

Table 3

Test Results

Numerous evaluations were made in two-pack polyurethanes with acrylic and polyester polyols, baking polyester-melamine, and acrylic-melamine systems. Films containing the new silicone-modified acrylate additive exhibit a hydrophobic and oleophobic surface with several other interesting properties.

Figure 9 / Dusting Coating Surface with Red Iron Oxide. The Left Side is the Control, the Right Side Contains the Additive.

Surface Energy/Surface Tension of the Dry Film

A physical parameter used to characterize the surface's cleanability is the surface energy or surface tension of the cured coating, consisting of a "polar" and a "disperse" component. Surface energy reduction capabilities of the new silicone-modified crosslinkable acrylate additive were evaluated in a two-pack PU coating. According to these test results, the overall surface tension of the dry film is only reduced approximately 15% by the silicone-modified acrylate additive. However, the polar component of the surface tension is reduced by more than 97%. This reduced polar component of the surface tension remains unchanged even after surface washing with 80 deg C hot water -- an excellent indication of its permanence (see Figures 7-8).

Figure 10 / After Rinsing with Water, the Right Side of the Panel is Clean.

Surface Tension of Liquid Coatings

The surface tension reduction capabilities of the new additive in liquid coatings are very similar to those of polyether-modified dimethyl polysiloxanes. Table 2 shows the (static equilibrium) surface tension reduction by the new additive in comparison to a conventional polyether-modified silicone typically used as a slip, substrate wetting and anti-cratering additive. Due to the similarity of the surface tension values, the new additive can provide not only easily cleaned surfaces, but is also suitable for improving substrate wetting and anti-cratering properties of liquid coatings.

Figure 13 / Different Wetting Behavior or a Felt Pen on a Conventional Surface (Left) and on a Surface With the New Additive (Right)

Dirt/Dust-Release Properties

The dirt-releasing properties of a coating's surface can be evaluated by rating the degree of removal of solid particulates on the coating's surface. A common and crucial test is to contaminate the coating surface with red iron oxide or carbon black pigment and then evaluate the surface's ability to be cleaned by a gentle rinse with detergent-free tap water.

Table 3 shows the dirt-releasing properties of various baking and air-drying OH-crosslinkable systems. According to the results, the incorporation of the new silicone-modified polyacrylate provides complete and easy removal of contaminating particles on the surface in all three systems.

Figure 14 / The Felt Pen Marks on the Right Side can be Easily Removed by Wiping with a Clean, Dry Cloth.

Anti-Fouling Properties

Low-energy surfaces may provide a certain level of resistance to fouling by marine organisms such as barnacles, slime, seaweed, etc. In order to investigate possible anti-fouling properties, a two-pack acrylic-polyurethane coating without anti-fouling agents was formulated with 2, 4 and 6% silicone-acrylic additive, applied onto suitable substrates, cured and subjected to static seawater fouling tests in Singapore, 60 cm below the surface for two months.

Results show that the silicone-modified acrylate additive cannot completely prevent fouling, but significant changes in the composition of fouling organisms indicate that this approach can be a basis for future developments.

The amount of barnacles, slime and seaweed growth on the coating surface was lowest at approximately 4% additive (see Figure 11). However, contamination by fungus appears to peak at 4% additive. The increased fungal growth is not a concern because it is easily removed. Although the total amount of foulant (slime, mussels, barnacles, seaweed, fungus, worms) was only reduced by 13%, the compositional change of the fouling organisms and ease of removal of those organisms is highly indicative of the potential benefits of this approach. Keep in mind that this was a static test; in actual use conditions, there would be a steady flow of sea water to help keep the surface clean.

Anti-Graffiti Properties

Resistance to graffiti can be tested using various types of permanent marker pens and evaluating their ease of removal by wiping with a dry clean cloth. Another common technique is to test the removal of spray paint (aerosol), the most widely used medium for graffiti, from surfaces with high-pressure water or steam. The silicone-acrylate additive provides in both tests very impressive improvements in the anti-graffiti properties of coatings, even with the most persistent graffiti.

However, excellent resistance to graffiti severely limits recoat adhesion. This additive is only recommended for those applications not needing recoatability. Recoating is only possible after thorough surface sanding, or following prolonged exterior exposure and subsequent erosion of the upper surface of the coating.

Practical Experiences and Applications

Due to the described properties of the new additive, many interesting coatings with unique surface properties can be developed for new applications. Potential areas for this new technology are in the following.
  • Polyurethane coatings for buildings, facades, ceramic tiles of tunnels that are graffiti resistant (for easy removal of graffiti).

  • Polyurethane wood coatings for kitchen cabinets (for easy cleaning).

  • Baking alkyd-melamine and polyester-melamine coatings for household appliances (for easy cleaning and scratch resistance).

  • Polyurethane coatings with improved foulant releasing properties due to the low surface energy (anti-fouling for higher speed vessels).

  • Polyurethane coatings for consumer electronics with easily cleaned and scratch-resistant surfaces.

  • Interior coatings for metal drums / pails / other technical metal packaging containers to provide more complete drainage of the contents.


Summary

A new silicone-modified crosslinkable acrylate additive has been developed that provides surfaces with easy cleaning characteristics along with many other interesting properties in OH-crosslinkable systems. Best results are obtained with 4-6% additive on liquid coating weight (1-1.5% active substance on total).

Acknowledgement

The authors would like to thank Kansai Paint in Singapore for its valuable support in performing and evaluating the anti-fouling test results.

Figures 1-4 are used in this paper with the kind permission of Prof. W. Barthlott and Dr. C. Neinhuis (University of the City of Bonn, Germany).

This article is based on a paper presented at the 30th Annual International Waterborne, High-Solids, & Powder Coatings Symposium[R] in New Orleans.

For more information on additives, contact John W. Du, BYK-Chemie USA, 524 South Cherry St., Wallingfor, CT 06492; e-mail jdu@bykchemieusa.com.

References

1 Barthlott, W. & Neinhuis, C., 1997: The Purity of Sacred Lotus or Escape From Contamination in Biological Surfaces, Planta 202, 1-8.
2 Neinhuis, C. & Barthlott, W., 1997: Characterisation and Distribution of Water-Repellent, Self-Cleaning Plant Surfaces. Annals of Botany 79, 667-677.

Links

  • BYK-Chemie USA

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Paint and Coating Market Reports
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Paint and Coating Market Reports
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

Akzo, SW, Nippon Logos

AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

BASF SE Logo

BASF Announces Strategic Business Sale

AkzoSWNipponEndTalks

Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Inside the AI Shift in Coatings - See the article now

Related Articles

  • Micronized Wax to Enhance Surface Protection of Water-Based Wood Coatings.jpg

    Micronized Wax to Enhance Surface Protection of Water-Based Wood Coatings

    See More
  • Borchers OM Group Bring New Additive Technology to ACS

    See More
  • U.S. Zinc Implements New Guidelines and Tools to Enhance Customer Service

    See More

Related Products

See More Products
  • Handbook of Adhesives and Surface Preparation

  • marketsandmarketslogo.jpg

    Pipe Coatings Market by Surface (Internal and External)...

  • Adhesion, Surface Aspects & Coatings Defects (Virtual Course - 10/22/26)

See More Products

Related Directories

  • BASF Corp., Dispersions, Resins & Additives

    BASF offers a strong portfolio of industry-leading additives for the Coatings Industry to deliver eco-efficient solutions that meet performance requirements. The BASF Performance and Formulation additives portfolio encompasses a technology base of dispersing agents, wetting agents and surface modifiers, defoamers, rheology modifiers, film forming agents, antioxidants, light stabilizers and UV absorbers.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing