UV-Curable Polyurethane Acrylate Dispersions Compared to 100%-Solids



The use of waterborne UV-polyurethane dispersions (UV PUDs) has been growing in the areas of wood furniture, kitchen cabinets and automotive products. Typically supplied at 30-40% solids, these UV PUDs are used to formulate sprayable coatings that produce low(er) dry coat weights than can be achieved with 100%-solids UV coatings at room temperature.

Performance properties have been determined using model formulations based on UV PUDs and standard oligomers diluted with butyl acetate. Mechanical properties and chemical resistance of UV PUDs are similar or better than those obtained with standard oligomers, with the additional benefit of physical drying that leads to a tack-free film before UV cure while minimizing VOC generation.



Table 1

Introduction

The increased use of waterborne UV-curable coatings is due to improved product performance, ease of handling and application benefits, and an ever-increasing awareness and concern for the environment. Correspondingly, there is an increasing interest in comparing the performance characteristics of waterborne UV-curable resins to those obtained with standard, 100%-solids UV-curable materials.

Although the benefits of high line speed associated with UV curing are reduced when waterborne UV-curable coatings are employed (water evaporation becomes the slow step in the process), use of these materials is increasing due to other characteristics that cannot be easily obtained with standard UV-curable systems. Some of the advantages of waterborne UV-curable coatings include:1,4,6-8

  • the absence of low-molecular-weight monomers, thus reducing the irritability of the formulation and eliminating their detrimental effect on the properties of the cured coating;
  • thickness control without VOC emission, an important feature in spray applications;
  • ease of design of low-gloss coatings, requiring lower levels of matting agents; and
  • physical drying of the coating, allowing handling and light sanding before UV cure.
This study compares the performance properties of coatings based on waterborne UV-curable resins with those obtained using resins employed to formulate 100%-solids UV-curable systems. Four UV-curable polyurethane dispersions (UV PUDs) are compared with one aromatic (ARUA) and two aliphatic urethane acrylates (ALUA) recommended for use in flooring and furniture applications. All five products are manufactured by Cytec.

Table 1 presents the properties of the products. UCECOAT® 7772, 7849 and 7631 are aliphatic PUDs that give a tack-free film after water evaporation and prior to UV cure. Cured films based on UCECOAT 7772 are characterized by high surface hardness as well as stain and chemical resistance; 7849 imparts flexibility while maintaining stain and chemical resistance; and  7631 has been designed for exterior applications and is characterized by superior weatherability combined with good mechanical properties and chemical resistance.

UCECOAT 7177 is characterized by good substrate and pigment wetting properties. Cured coatings based on this oligomer show surface hardness with high stain and chemical resistance. The film produced after water evaporation is not tack-free before UV cure.

EBECRYL® 4827 is an aromatic urethane acrylate that imparts high flexibility. EBECRYL 284 and 4833 are aliphatic urethane acrylates with good scratch and abrasion resistance, and they are commonly used in flooring applications.

 



Experimental Procedures

Coatings prepared for testing contained 34% resin and 2% ADDITOL® HDMAP as a photoinitiator, the balance being water in the case of UV PUDs and butyl acetate for the 100%-solids UV curable resins.

Formulations were applied with a #10 drawdown bar on transparent vinyl, cold roll steel panels, unlacquered opacity charts and wood veneer (maple and oak). Butyl acetate or water was evaporated at 65 ºC for 10 minutes, and the sample was cured with a Fusion brand EPIQ 6000 unit using two H lamps operated at 600 watt/inch. Typical energy density employed was 1 J/cm2. Thickness of the cured coating was 0.3 mil, measured with a Gardco brand Minitest 100N gauge.

Adhesion to the substrates was determined by the cross hatch method using 3M’s 610 Scotch® brand tape,  gloss at 20º and 60º with BYK Gardner’s micro-TRI-gloss meter and color coordinates with a BYK Gardner Color Guide. Pencil hardness was measured on steel panels using Staedler’s Mars 780 pencil set, flexibility with a conical mandrel, and reverse impact resistance with a BYK Gardner brand impact tester using a 2-lb weight.



Abrasion resistance was determined on opacity charts with a Taber brand Abraser using CS-17 wheels and 1000-g weights. The weight loss after 100 cycles is used as a measure of abrasion resistance. Taber scratch resistance was measured on opacity charts with Taber’s 502 Shear Scratch Tester as the applied weight required to break through the surface. Resistance to MEK was determined by rubbing the surface of the cured coating with cheesecloth saturated with solvent and attached to the head of 2-lb ball-peen hammer.

Stain resistance was determined by placing a drop of staining material on the surface of the cured coating, covering with watch glass to prevent evaporation, and allowing to stand for 24 hours prior to inspection (1 hour for mustard). After removing the staining material, the surface was inspected visually. A more quantitative measure was obtained for mustard and coffee by determining the CIE L*a*b* color coordinates with BYK Gardner’s Color Guide spectrophotometer.

Tensile properties were measured on free films with an Instron brand 4467 tester.  Free films were prepared by applying the formulations on polyester films using 5 mil spacers. Butyl acetate and water was evaporated at room temperature for 24 hours, after which the samples were placed at 65 ºC for 48 hours prior to curing and processing.



Figure 2

Results and Discussion

All coatings had excellent adhesion to vinyl, maple and oak and good adhesion to steel and unlacquered opacity charts. Pencil hardness was between 4H and 6H, and all coatings showed good flexibility and impact resistance.

Table 2 shows results for MEK resistance, Taber scratch and abrasion resistance of the cured films. The aromatic urethane acrylate shows the poorest performance properties of the series, whereas MEK and scratch resistance of the UV PUDs are higher than those obtained with the standard aliphatic urethane acrylates.

The lower abrasion resistance observed for the UV PUDs is attributed to lower resiliency of these resins. As Figures 1 and 2 show, the UV PUDs show similar tensile strength to the ALUAs but significantly lower elongation. The result is lower film toughness and reduced abrasion resistance.



Figure 3

Coatings based on UV PUDs produce films with lower gloss than those based on standard UV resins, the differences being more significant at 20º, as seen in Figures 3 and 4. UCECOAT 7772 gives the lowest gloss and requires lower levels of matting agent to obtain a matt coating. No matting agent is required with UCECOAT 7772 to obtain gloss at 20º in the 15-20 range.



Table 3

Table 3 shows the chemical resistance of cured coatings to a variety of staining materials. This qualitative test indicates that UCECOAT 7772 has the highest chemical resistance and the aromatic urethane acrylate-based coating has the lowest. Stain resistance with mustard and coffee has been quantitated by measuring the change in the CIE L*a*b* color coordinates upon exposure. These materials are the strongest staining materials that are employed in the battery of tests required to obtain certification by the KCMA.

Figure 5 shows the change in the CIE b* coordinate and allows a better visualization of the differences in stain resistance between the UV PUDs and standard UV-curable materials. It should be noted that a change of less than 1 unit in the CIE b* coordinate is virtually undetectable by the naked eye.



Figure 4

In review of the comparative data, the selected UV PUDs (UV-curable polyurethane dispersions) evaluated displayed excellent stain resistance qualities and Taber scratch resistance. These properties are in great demand in a variety of markets and offer added value to the end users. Due to their lower total solids, the UV PUDs would also add ease in handling and end-use application over the undiluted 100%-solids UV systems.

The UV PUDs evaluated in this study displayed equal or better performance properties than the selected aliphatic urethanes, especially in the area of stain resistance, and better performance characteristics than the aromatic urethane.

In overall visual appearance, the UV PUDs exhibited lower gloss than the 100%-solid UV systems, especially at 20º. This low-gloss characteristic is an asset for product lines requiring low sheen while minimizing the level of flattening agents.



Figure 5

Conclusions

The UV PUDs evaluated in this work showed similar or better performance properties than the standard UV-curable urethane acrylates. The viscosity of the coating can be adjusted with water, and the thickness of the cured coating can be easily controlled without VOCs or HAPs emission, all of which are important characteristics in spray applications such as for kitchen cabinets.

For more information, visit www.cytec.com.

Angela Carmack | Cytec Industries, Inc., Smyrna, GA
Marla de Lombard-Watts | Cytec Industries, Inc., Smyrna, GA
Oscar Valdes-Aguilera | Cytec Industries, Inc., Smyrna, GA
You must register or login in order to post comments.

Multimedia

Videos

Image Galleries

Podcasts

PCI Top 5 - January 12, 2012
PCI's Podcast series on the five most e-mailed/shared articles and stories for the week.

More Podcasts

THE MAGAZINE

PCI Magazine

February 2012 cover

2012 February

PCI's new issue is now available. Check it out!

TABLE OF CONTENTS SUBSCRIBE

Coating Technology

What resources do you refer to when learning about coatings technology?
See Poll Results Poll Archive

THE PCI STORE

Power Coatings
CD Verison: Powder Coatings - Foundation for the Novice Formulator by Kevin Biller for $29.95 plus shipping
ON CD - Powder Coatings have been the fastest growing finishing technology for the past 30 years. In spite of this tremendous growth and the technology advances that come with it, very few technical tools have been provided for the formulator.
More Products

Clear Seas Research

Clear Seas ResearchWith access to over one million professionals and more than 60 industry-specific publications,Clear Seas Research offers relevant insights from those who know your industry best. Let us customize a market research solution that exceeds your marketing goals.

Virtual Brochures

PageCollageClick to the Virtual Brochures page to view multiple catagories that list downloadable product literature from leading industry suppliers.

STAY CONNECTED

Facebook Twitter  LinkedIn