Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Waterborne Parquet Coatings Based on Crosslinked Polyurethane Dispersions

January 31, 2002
Figure 1:The Structure of Polyurethanes
Compared with solventborne systems, traditional waterborne parquet coatings lack various properties such as scuff- and chemical resistance. Several approaches have been investigated in the past to overcome these drawbacks, but many of them were not totally successful. New generations of raw materials for manually applied parquet coatings (waterborne one- and two-component) and industrial application (UV-curing parquet coatings) were developed. Each represents remarkable progress in its particular field of application. These new systems are discussed with respect to their properties and polymer structure.

Characteristics of Polyurethane Coatings

All polyurethane coating systems are produced by the isocyanate-polyaddition process in which isocyanates and suitable co-reactants are combined to produce polymers containing urethane groups (see Figure 1).

The characteristic feature of polyurethanes is their chain structure of hard and soft segments. The hard segments have a large number of urethane groups that crosslink physically through the formation of hydrogen bridges. While the hard segments can form crystalline structures, the soft segments are comparatively mobile. From the combination of these attributes in the same molecule, the tough but flexible property profile of polyurethane coatings is achieved.

Despite the advantages of waterborne polyurethane coatings based on polyurethane dispersions (PUDs) for parquet floor coating application, there are some shortcomings about current commercially available systems.

  • Low black heel mar resistance
  • Inadequate storage stability of the dispersions and the formulated coating
  • Poor chemical resistance under severe exposure
  • Inadequate grain accentuation of the wood substrate
To overcome these shortcomings and develop waterborne systems with improved properties that can rival traditional parquet floor coatings, three possibilities of incorporating chemical crosslinking into polyurethane dispersions were investigated: oxidative crosslinking, polyisocyanate crosslinkers and radiation curing.

Figure 2:AFM Photography of a Film from a Polyurethane Dispersion and Polyisocyanate Crosslinker; Tapping Mode; 7 d after Application

Fatty Acid Modified Polyurethane Dispersions - Oxidative Crosslinking

Despite their physical crosslinking by way of hydrogen bridges, coatings using PUDs are, to a certain extent, thermoplastic. As a result, the heel marks left behind by hard shoe soles can often lead to irreversible damage. These heel marks virtually burn into the film.

It seemed logical to solve this problem by introducing an additional chemical crosslinking process. The first option is to introduce the oxidative crosslinking mechanism by way of drying oils - a method that has already proved itself in the parquet segment. Many attempts have already been made in this direction to improve the overall properties of waterborne coatings. In most cases, however, the result turned out to be an inadequate compromise. The improved black heel mar resistance (BHMR) was achieved at the expense of the abrasion resistance or the yellowing resistance.

The introduction of drying oils into the polymer structure of an aqueous polyurethane dispersion can be carried out in a variety of ways. To maintain the desired properties of the waterborne PUD coating, it is important to introduce a minimal amount of drying oil. To achieve a crosslinking effect that extends beyond the particle interfaces, even with low oil content, the crosslinking unit must be very mobile. This means that the fatty acid should be incorporated in the soft segment of the polyurethane. In the case of high-molecular-weight PUD coatings, very low oil content (less than 10%) is enough to obtain the desired properties. However, the introduction of crosslinking components into the soft segment leads to a reduction of the elasticity and thus decreased abrasion resistance. This can be compensated through careful selection and arrangement of the high-grade components such as cycloaliphatic diisocyanates and soft segments with excellent mechanical properties.

A careful choice of the raw materials also makes it possible to formulate a PUD coating with excellent storage stability. After four weeks at 50 degC or even after three freeze/thaw cycles between -10 degC and +20 degC, the properties are virtually the same as they were at the beginning. This also applies to other critical parameters such as antifoam stability and viscosity.

The resulting high-molecular-weight PUD, with less than 5% co-solvent, guarantees rapid drying while low mean particle size leads to high wet film transparency and also accentuates the grain.

This new development permits the formulation of one-component aqueous coatings with excellent black heel mark resistance, good chemical resistance, improved appearance and grain accentuation. At the same time, yellowing and abrasion resistances are similar to that of the traditional aliphatic waterborne systems.

Figue 3: Incorporation of Radiation-Curing Units into a Polyurethane Dispersion

Waterborne Two-Component Polyurethane Coatings

Aqueous two-component polyurethane systems are a young class of binders for parquet coatings. In this market, a two-component coating will only be accepted if its overall properties are significantly better than those of a one-component system. Other key factors for the acceptance of a two-component system are ease of mixing, ease of application and acceptable potlife.

Good results are obtained when a high-molecular-weight polyurethane dispersion is used as Component A. Even without a crosslinking agent, the PUD produces a high quality finish. The properties of Component A contribute certain overall coating properties such as hardness and drying rate. The incorporation of Component B, the polyisocyanate crosslinking agent, produces a level of chemical and mechanical resistance previously unattained in waterborne coatings.

For manual application, it is essential that the curing agent can be easily incorporated into Component A. People have been using hydrophilically modified polyisocyanates as the crosslinking agents for this purpose.

When designing a crosslinker for waterborne coatings, the level of hydrophilicity must be adjusted to achieve target properties because:

  • A high (but not excessive) content of hydrophilic groups simplifies incorporation of the crosslinker,

  • An excessive content of hydrophilic groups, on the other hand, impairs the chemical resistance.
The first generation of waterborne two-component polyurethane parquet sealers consisted of a combination of component A and a polyisocyanate with a comparatively low hydrophilic content. As a result, the crosslinker did not become sufficiently homogenized during manual mixing, and the parquet finish frequently turned out rather cloudy. Therefore, the use of this technology was limited to matte and, in some cases, silk-gloss finishes. Our aim was therefore to develop a curing agent for waterborne two-component high-gloss polyurethane coatings that could be easily incorporated under practical conditions. This required a more finely dispersed polyisocyanate with optimal level of hydrophilic modification.

A new generation of hydrophilically modified polyisocyanates was therefore developed.

In comparison with the traditional types in which the hydrophilic group is linked by way of urethane bonds to the basic polyisocyanate matrix, the new generation contains allophanates that are formed from a urethane further reacting with isocyanate. At the same level of hydrophilic modification, an allophanated polyisocyanate disperses far more finely in water than the traditional urethane.

This simple modification to the crosslinker structure significantly affects the properties of the two-component system. Our new crosslinker for waterborne parquet coatings can be easily dispersed simply by shaking the container. Resultant particle sizes are in the range of ~100 nm, which are also the typical values for polyurethane dispersions. Therefore, for the first time, thorough mixing under parquet coaters?ractical conditions is now possible.

An analysis of such coatings by 13C-NMR spectroscopy has shown that the polyisocyanate reacts (for the most part) with moisture to form the polyurea network. The crosslinking principle is thus similar to that of conventional, moisture-curing polyurethane. The film morphology of an aqueous two-component polyurethane coating of this kind can be illustrated with the aid of atomic force microscopy (AFM) in the tapping mode. In the cured aqueous two-component polyurethane coating, a matrix of polyisocyanate surrounds the polyurethane particles, of which there is a large surplus. This matrix is very soft, but highly crosslinked. Even in the cured film, the polyurethane particles from Component A can still be individually recognized under AFM. These particles are significantly harder than the polyisocyanate matrix. In other words, an additional 'overstructure' is created in the film as well as the described hard/soft morphology of the polyurethane molecules. Due to the small particle size of the initially water dispersed polyisocyanate there are no large domains of polyisocyanate in the film. In the case of previously used polyisocyanates, these large domains tend to result in turbid films after drying.

A combination of our new polyisocyanate with a high-gloss Component A produces a highly resistant, high-gloss waterborne two-component polyurethane coating (see Table). Upon incorporation of the crosslinker, the coating system has a potlife of about five hours and still yields consistent properties. After this time, the most significant change is gloss reduction.

Table 1

Radiation-Curing Polyurethane Dispersions

While polyurethane dispersions dominate the market in the field of environmentally friendly parquet coatings for manual application, they are not commonly used in ready-made parquet floors.

Ready-made parquet is roller coated primarily with unsaturated acrylates. The elimination of the drying section for solvent removal and the fast curing speed of the radiation-curing process save a considerable amount of time. Urethane acrylates in particular can also satisfy the stringent requirement of abrasion resistance.

However, the disadvantages of this technology include the following.

  • The high degree of crosslinking is the main reason for the high shrinkage of such coating systems. This shrinkage often leads to adhesion problems between radiation-cured coatings and the wood substrate.

  • The flexibility, even of high-grade urethane acrylates, does not attain the level of aqueous PUDs.

  • It is more difficult to down-gloss these high-solids systems than it is with waterborne coatings.

  • The reactive thinners currently used are often a concern for an occupational hygiene point of view.

  • The roller application of 100% systems often produces a rather inferior finish.
The obvious course, therefore, seemed to be to combine the key advantages of radiation curing with the attributes offered by the PUD chemistry. One way to achieve this is to incorporate a certain proportion of polymerizable double bonds into aqueous PUDs without sacrificing the toughness as well as flexibility.

These UV-curable aqueous dispersions have a molecular weight that is many times higher than that of traditional systems consisting of an unsaturated acrylate and a reactive thinner. This is why the waterborne systems need much less radical crosslinking to obtain the desired properties. This means:

  • The toughness and flexibility of polyurethanes are largely retained, which leads, for example, to high abrasion resistance and elongation.

  • The shrinkage is much lower; aqueous radiation-curing polyurethane dispersions are therefore ideal as adhesive primers in a parquet coating system for industrial application.

  • The photoinitiator requirement is lower - an important cost factor.
The need of a reactive thinner is eliminated in these systems.

The advantages of these systems over 100%-solid UV-curing coatings are that it is much easier to obtain a matte finish and that they can be applied by curtain coating. Thus the aqueous, radiation-curing systems are also ideal for the topcoat for ready-made parquet flooring.

Their inherent disadvantage compared with the 100%-unsaturated acrylates is the presence of water. Water has to be removed from the film before UV curing. As aqueous coatings become more popular, highly effective drying equipment has been developed that can be used for such applications.

The optimum coating system for ready-made parquet flooring would be as follows.

  • Apply an adhesive primer with good penetration and wetting properties, based on a radiation-curing aqueous dispersion, by roller. This adhesive primer alone has already produced good results for the pretreatment of oiled parquet flooring.

  • Limit the number of flash-off zones. This would be followed by two or three coats of a 100%-solid urethane acrylate, free of reactive thinner, also by roller.

  • To ensure maximum quality, an aqueous topcoat is the best choice. For optimum appearance, a curtain coating machine would be used to apply the radiation-curing PUDs, set at the desired gloss level.

    Summary

    Because of their outstanding overall property profile, aqueous polyurethane dispersions are the most popular class of binders for environmentally friendly parquet finishes. Proven technical advantages over conventional parquet coatings are their high abrasion resistance, rapid drying and their minimal detrimental impact on the environment.

    A low level of oxidative crosslinking is enough to significantly reduce the thermoplasticity of one-component waterborne coatings. This leads to greatly improved black heel mark resistance. With the development of fatty acid modified PUD, it is also possible to achieve excellent abrasion and yellowing resistances, good storage stability and improved grain accentuation.

    It is known from conventional one- and two-component polyurethane coatings that crosslinking via polyisocyanates brings a significant additional improvement in the resistance properties. With our new generation of water-dispersible polyisocyanates with more effective chemical linkage of the hydrophilic groups, it has become possible for the first time to formulate easy-to-apply waterborne two-component polyurethane coatings with a high surface gloss.

    The newly developed UV-curable PUDs marries the advantages of radiation curing technology and aqueous PUD technology to achieve the desired properties including various gloss levels with high throughput and excellent adhesion to the wood substrate.

    We are convinced that polyurethane dispersions will continue to gain popularity in the field of industrial parquet coatings. The enormous range of structural parameters makes it possible to develop a tailor-made solution for just about any coating system.

    This article is based on a paper presented at the International Waterborne, High-Solids and Powder Coatings Symposium February 21-23, 2001, in New Orleans. The symposium is sponsored by The University of Southern Mississippi Department of Polymer Science.

    For more information on polyurethane dispersions, contact Christoph Irle, Bayer Hispania S.A., Pau Claris, 196, 08037 Barcelona, Spain; or Bob Wade, Bayer Corp., Coatings and Colorants Division, 100 Bayer Road, Pittsburgh, PA 15205-9741; phone 412/777.2871; fax 412/777.2084; visit www.bayerus.com; e-mail bob.wade.b@bayer.com; or Circle Number 90.

    Links

    • Bayer Corp.
  • Share This Story

    Looking for a reprint of this article?
    From high-res PDFs to custom plaques, order your copy today!

    Recommended Content

    JOIN TODAY
    to unlock your recommendations.

    Already have an account? Sign In

    • pci1022-Kinaltek-Lead-1170.jpg

      A Novel Pigment Production Technology

      Following an extensive R&D program that demonstrated...
      Paint and Coating Pigments
      By: Jawad Haidar and Nitin Soni
    • pci global top 10

      2025 Global Top 10: Top Paint and Coatings Companies

      The following is PCI’s annual ranking of the top 10...
      Global Top 10 and PCI 25
      By: Courtney Bassett
    • 2025 pci 25

      2025 PCI 25: Top Paint and Coatings Companies

      PCI's annual ranking of the top 25 North American paint...
      Paint and Coating Market Reports
      By: Courtney Bassett
    You must login or register in order to post a comment.

    Report Abusive Comment

    Manage My Account
    • eMagazine
    • Newsletters
    • Online Registration
    • Subscription Customer Service

    More Videos

    Sponsored Content

    Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

    close
    • wooden kitchen set and shelving
      Sponsored bySirca North America

      Leveraging Coatings to Meet ESG Goals in Manufacturing

    • man woodworking in workshop
      Sponsored byGemini Industries, Inc.

      Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

    Popular Stories

    Akzo, SW, Nippon Logos

    AkzoNobel Rejects Cash Offer From Nippon Paint, Sherwin-Williams

    BASF SE Logo

    BASF Announces Strategic Business Sale

    AkzoSWNipponEndTalks

    Nippon Paint, Sherwin-Williams End AkzoNobel Pursuit

    POB-Point-and-Shoot

    PCI Buyers Guide

    Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

    Start your RFP

    Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

    Find Suppliers

    Events

    September 4, 2025

    N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

    ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

    September 15, 2026

    Coatings Trends & Technologies Summit

    The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

    View All Submit An Event

    Poll

    Longest-running laboratory experiment

    What is the longest-running laboratory experiment?
    View Results Poll Archive

    Products

    Automotive Paints and Coatings, 2nd Edition

    Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

    See More Products
    Inside the AI Shift in Coatings - See the article now

    Related Articles

    • Crystallinity of Coatings Based on Polyvinylidene Fluoride

      See More
    • High-Performance Coatings Based on Hybrid Organic-Inorganic Polymers

      See More
    • pci0322-Troy-473388139-1170.jpg

      New Engineered Polysaccharides as Sustainable Performance Additives in 1K Water-Based Polyurethane Dispersions

      See More

    Related Products

    See More Products
    • biopolymer.jpg

      Biopolymer-Based Films and Coatings Trends and Challenges

    • Waterborne Polymers and Film Formation (Virtual Course - 7/23/26)

    See More Products
    ×

    Keep the info flowing with our eNewsletters!

    Get the latest industry updates tailored your way.

    JOIN TODAY!
    • RESOURCES
      • Advertise
      • Contact Us
      • Directories
      • Store
      • Want More
      • Manufacturing Division
    • SIGN UP TODAY
      • Create Account
      • eMagazine
      • Newsletters
      • Customer Service
      • Manage Preferences
    • SERVICES
      • Marketing Services
      • Reprints
      • Market Research
      • List Rental
      • Survey & Sample
    • STAY CONNECTED
      • LinkedIn
      • Facebook
      • Youtube
      • X (Twitter)
    • PRIVACY
      • PRIVACY POLICY
      • TERMS & CONDITIONS
      • DO NOT SELL MY PERSONAL INFORMATION
      • PRIVACY REQUEST
      • ACCESSIBILITY

    Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

    Design, CMS, Hosting & Web Development :: ePublishing