  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!
Names in the News

Steve Hutton Joins Board of HMG Paints

Steve Hutton and Jonathan Falder
October 28, 2020

MANCHESTER, UK — HMG Paints has appointed Steve Hutton to the company’s Board of Directors. This marks the second appointment to the board in the company’s 90th year of business, with Jonathan Falder joining the board in January.

Hutton joined HMG Paints in 2001 and is the third generation of the Hutton family to work at HMG. He is the second member of the family to be appointed as a Director and joins the board exactly six years after his father Len Hutton, who is the Production Director.

“The people of HMG are what makes HMG the company it is. We are extremely proud that generations of families have worked at HMG, and I’m delighted to welcome Steve to the board of HMG,” said John Falder, Managing Director. “It is very true that we are custodians of the business for the next generation who are going to create something better. I believe the young people that we invest in today will go on to have long careers and lead HMG Paints in the future and the appointments of Steve and Jonathan are testament to that.”

Steve Hutton is also in the final stages of his postgraduate Doctorate of Philosophy (DPhil) at Lancaster University where he also completed his MSC in 2016. He has experience with many HMG departments, including the Colour Laboratory, Quality Control, several manufacturing departments, Warehousing and Logistics, and then more recently, Production Planning, giving him the background and experience for this new role.

KEYWORDS: Paint and Coating Manufacturers personnel announcements

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • Double exposure of creative chemistry concept on laptop background, research and development concept

    Inside the AI Shift in Coatings

    Industry leaders share real-world examples of how AI is...
    Architectural Coatings
    By: PCI Editorial Staff
  • Global Top 10 and PCI Logo

    2026 Global Top 10: Top Paint and Coatings Companies

    See how the world’s largest paint and coatings companies...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • The 2026 PCI 25

    2026 PCI 25: Top Paint and Coatings Companies

    See how North America's largest paint and coatings...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

Popular Stories

PCI 2026 Voices from the Top eBook cover

eBook | 2026 Voices from the Top

The 2026 PCI 25

2026 PCI 25: Top Paint and Coatings Companies

AkzoNobel, Nippon

Nippon Paint Returns With €7.5B Proposal for AkzoNobel Business

The PCI 25 Annual Revenue Rankings

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

September 15, 2026

Coatings Trends & Technologies Summit

The Coatings Trends & Technologies (CTT) Summit is an annual conference for both liquid and powder coatings formulators and manufacturers to discuss innovations in coatings technology. This event combines high-quality technical presentations, a resource-rich exhibit hall, and dedicated networking opportunities to connect scientific minds, foster innovation, and cultivate game-changing new ideas!

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
PCI Coat It! Podcast

Related Articles

  • Paul Sheppard of HMG Paints

    Paul Sheppard of HMG Paints Becomes OCCA President

    See More
  • Managing Director of HMG Paints Appointed BCF President

    See More
  • Thomas W. Handley Joins Board of H.B. Fuller

    See More

Related Products

See More Products
  • Failure Analysis of Paints and Coatings, Revised Edition

  • Automotive Paints and Coatings, 2nd Edition

See More Products

Related Directories

  • Titan

    As a leader in spraying technology, Titan manufactures and markets a full line of professional-grade paint sprayers for applying a variety of coatings.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing