Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!

Burnish Resistant, Ultra-Durable Matte Powder Coatings

October 2, 2000
As the 1990s come to a close, the U.S. powder coating industry continues to grow at more than 10% each year.1 The environmental advantages powder holds over conventional coatings continue to be amplified, as the costs of regulatory compliance continue to increase for metal finishers. Perhaps just as importantly, raw-material suppliers have continued to develop novel materials, thereby allowing powder coatings to compete in market niches, previously the exclusive domain of liquid coating technology. Two examples are so-called low-temperature and UV-curable powders for use on thermally sensitive substrates.

Another niche area in powder technology is that of matte finish powders. Matte powder coatings are popular due to their excellent physical and aesthetic properties. They can hide defects or irregularities in metal surfaces, and add value to consumer products. Applications for these powders include lighting fixtures, automotive trim parts, lawn furniture and architectural extrusions.

Many formulating techniques and chemistries have been developed for matte powder coatings over the last 15 years that allow for a range of appearance and film characteristics.

Epoxy and epoxy-polyester matte powders have been commercialized and have a strong track record in metal finishing.2 However, their poor weathering resistance has previously limited their use to indoor applications. This article will emphasize new developments in weatherable matte finishes, with a focus on “ultra-durable” low-gloss powder coatings.

Weatherable Matte Powder Coatings

Polyurethane chemistry is used for weatherable matte finishes. Low-gloss powders are produced by blending two or more OH-functional polyester resins, which have widely varying functionalities.3 These resins are cured with a blocked isocyanate, e.g., isophorone diisocyanate (IPDI) blocked with x-caprolactam. This approach is limited in practice in that the gloss may change markedly depending upon the formulator’s choice of isocyanate curative.4

Matte Polyester/Acrylic Technology

A matte finish curing mechanism has been recently commercialized by Reichhold using a bifunctional polyester (reactive COOH and OH groups) and glycidyl methacrylate (GMA) acrylic resin. The GMA acrylic crosslinks the polyester’s carboxyl groups, while isocyanate curative cures the hydroxyl groups, as before.5

The difference in cure speeds between the two reactions creates a micro wrinkling of the film, and the resulting matte effect. A simplified diagram of this three component system is shown in Figure 1.

The polyester/acrylic system can be formulated consistently into a matte finish with excellent mechanical properties. Tables 1 and 2 show a formulation and application data for a black powder coating.

Even with this novel crosslinking system and its excellent physical properties, further optimization can be realized. Two areas of technical interest are improvements in burnish resistance and exterior durability.

Burnish Resistance

In many finishing applications, handling and packaging of painted products can cause marring of the painted surface, creating rejects and increasing the cost to the metal finisher and ultimately the consumer. In matte-finished products, marring or burnishing usually result in a gloss increase.

Figures 2 and 3 show SEM photographs of a cured polyester/acrylic matte powder coating before and after a burnishing event. Although the naked eye can easily view an unacceptable burnish area, surprisingly, there is virtually no change in the coating surface structure when viewed with the microscope. This powder coating with a relatively high glass transition temperature (Tg = 57°C), may be too brittle to be resistant to scratching. While this polyester/acrylic retains other desirable properties such as impact and chemical resistance, it may not be suitable for applications that demand burnish resistance.

If softer, lower Tg polymers are substituted for the standard materials, one can observe quite different results, both visually and microscopically.

Figures 4 and 5 display SEM photographs of Tg-modified polyester/acrylic matte powders, before and after the burnishing event. While it is easy to see a change in the film structure under the microscope (circled area denotes damage, see Figure 5), virtually no damage can be seen by the observer.

The burnish resistance of the modified powder is excellent. Just as importantly, other polymer physical properties are retained. Modifications to the polyester and acrylic polymers are contrasted to the “first-generation” polymers in Table 3.

Exterior Durability

Automotive and architectural powder coating applications have demanding weatherability requirements. Particularly in the architectural arena, “standard” exterior weatherable powders often do not meet these stringent specifications.6 “Superdurable” powders, while meeting weathering requirements, can be difficult to matte.

Special monomers are required to develop polyester powder resins with excellent weatherability. When introduced into resins, these materials typically cause reduced flexibility. The new matte finish system does not display this problem; the acrylic polymer has been altered to help retain coating flexibility.

Accelerated testing indicates this new-generation matte system features better exterior durability than the matte powders being used now. Figure 6 illustrates the difference in color retention between currently available matte powders and the new generation polyester/acrylic. Approximately a three-fold decrease in color shift is observed in QUV-340A accelerated testing.

Lower Temperature Cure

As mentioned earlier, low-temperature cure powders are an area of new-development in powder coatings. Use of polyurethane technology has been limited by the high temperatures required to unblock the isocyanate groups. Novel isocyanate curatives have been recently introduced that offer the potential for reduced cure temperatures. Some of these compounds have been tested for the possibility of lowering the cure temperature of the bifunctional polyester/GMA acrylic. The combination, as demonstrated in Table 4, helps deliver matte finish and cure properties as low as 250°F (see Figure 7).

GMA Compatibility

Concerns about compatibility of GMA acrylic resins with other powder chemistries have persisted. However, empirical studies show that differences between two powders’ melt viscosity and surface tension are more important to good compatibility than simply chemistry differences.7

The polyester/acrylic matte illustrates this point. The majority of the powder formula is a polyester resin. The polyester’s melt viscosity dictates the powder viscosity. Since the resin viscosity is in the same range of other typical powder resins, contamination of other powders from the polyester/acrylic should not be expected beyond what would occur when any two other powder chemistries are mixed. Lab tests conducted according to Powder Coating Institute Test Number 2 reveal no cratering, pinholing or significant surface defects resulting from contamination of the polyester/acrylic in other powder chemistries.8

Conclusion

A new-generation polyester/acrylic powder coating matte offers several interesting features, including the following.

  • Excellent reproduceability of gloss,

  • Excellent resistance to burnishing,

  • Excellent weathering resistance without sacrifice of mechanical properties,

  • Possibility of low temperature cure and

  • Good compatibility with other powder chemistries.

This development should have a wide application range in the growing exterior durable powder coating market.

Acknowledgements

Several Reichhold team members contributed to the success of this development, especially Allen Burbank, Gail Harrison, Goro Iwamura, Alan Toman and Andrew Woo.

For more information on powder coating resins technology, call Reichhold at 800/431.1920 or 919/990.7500 outside the U.S. www.Reichhold.com; or Circl.

Links

  • Reichhold

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • colorful building exterior
    Sponsored byDow

    Insights into Exterior Architectural Coating Degradation: Bridging Accelerated and Natural Weathering

  • digital pigments
    Sponsored bySiltech

    The Fourth Dimension of Silicon: Siltech Q Resins

Popular Stories

Orange painted wooden surface with paint roller and message in white: "Your Feedback Matters"

AI-Powered Coatings

Blue River Coatings

Blue River Coatings Names New Chief Executive Officer

TiO2

Chemours Reaches Agreement to Sell Former Titanium Dioxide Site

pci academy

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

February 24, 2026

Implementing AI in Paints & Coatings: Doing It Right

This webinar is designed for Enterprise Paints and Coatings leaders (Innovation, R&D, Product, Production) tasked with introducing AI, whether they are unsure where to start or have already launched pilots but struggle to scale. Attendees will learn common pitfalls of AI adoption and how experienced partners enable confident, scalable, and measurable impact in global Enterprise organizations.

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
pci case ebook

PCI webinar

Related Articles

  • pci0422-Shepherd-609811204-1170.jpg

    Problem-Solving Pigments for Powder Coatings: Durable, Functional and Colorful

    See More
  • Global Demand for Cost-Effective and Durable Powder Coatings on the Rise

    See More
  • PPG Wins Federal Award to Develop Chemical-Agent-Resistant Powder Coatings

    See More

Related Products

See More Products
  • Powder Coatings Processing (Virtual Course - 6/25/26)

  • marketsandmarketslogo.jpg

    Metallic Powder Coatings Market by Process Type (Bonding, Blending, Extrusion)...

See More Products

Events

View AllSubmit An Event
  • March 12, 2025

    Revolutionize Matte Coatings with Multifunctional Additives

    On Demand Register now and join this webinar to understand the factors that are driving formulators to explore the next generation of matting agents and explore the latest additive technologies.
  • April 23, 2025

    A New Multi-Functional Silicone Emulsion for Durable Exterior Architectural Coatings

    On Demand We will focus on how this functional silicone additive can enhance coating performance over time, without sacrificing other desired properties such as incompatibility, surface blooming and poor dirt pickup that is seen with traditional silicone polymer-based additives.
View AllSubmit An Event

Related Directories

  • Micro Powders

    Micro Powders' additives solve problems and achieve unique coating surface effects including: slip, rub, abrasion, scratch resistance; gloss reduction, burnish resistance; water repellency; texture, tactile, and soft touch effects. We are leaders in creating innovative particle technologies, including natural/biodegradable grades and nanocomposite wax PTFE alternatives.
  • Micro Powders

    Micro Powders' additives solve problems and achieve unique coating surface effects, including slip, rub, abrasion, scratch resistance; gloss reduction, burnish resistance; water repellency; texture, tactile and soft touch effects. We are leaders in creating innovative particle technologies, including natural/biodegradable grades and nanocomposite waxes to replace PTFE.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media.

Design, CMS, Hosting & Web Development :: ePublishing