Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Join Today
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • PCI News Now
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Global Top 10/ PCI 25
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • COAT-IT! Podcast
    • Videos
    • PCI Store
    • eBooks
    • Sponsor Insights
  • EMAGAZINE
    • eMagazine
    • Archive Issues
    • Editorial Advisory Board
    • CONTACT
    • Advertise
  • JOIN!
Paint and Coatings AdditivesPaint and Coating Resins & PolymersWaterborne Coatings

New Engineered Polysaccharides as Sustainable Performance Additives in 1K Water-Based Polyurethane Dispersions

By Jorge Mok, Christian Lenges, Natnael Behabtu, Ibrahim Sendijarevic, Dr. Aisa Sendijarevic
pci0322-Troy-473388139-1170.jpg
Credit: LeoPatrizi, Creatas Video, via Getty Images
March 11, 2022

Polyurethanes today represent one of the most diverse class of polymers, finding uses in a broad range of applications across multiple industries. Numerous raw materials are being utilized today in this diverse material category to enhance and modify product performance. Innovation continues to not only target further product performance improvements but also increasingly focuses on the overall material sustainability with regard to environmental aspects driven by a circular economy framework.  

In the protective coatings market, the major initiative has focused on improving the emissions by replacing organic solvents as the carrier material with water. As a result, solvent-free, water-based polyurethane dispersions (PUDs) have been developed for a broad range of applications including wood coatings, leather and textile coatings, and metal coatings. To meet the sustainability objectives, PUDs have also been synthesized from renewable-based PO3G polyether polyols. In addition, PUDs with high renewable content have been produced from polyester polyols based on succinic, azelaic, sebacic and octadecanedioic acids.

More recently, enzymatic polymerization has been under development to convert sucrose to engineered alpha-1,3-polyglucose (glucan) materials with properties tailored for use in water-based PUD coatings. Alpha-1,3-polyglucose can be produced from sucrose using a biocatalyst from the general class of glucosyltransferases (GTF), for example isolated from Streptococcus salivarius. These alpha-1,3-polyglucose systems are found in nature (for example from mushrooms) but are isolated here directly from a scalable bioprocess.

Representative structure of alpha-1,3-glucan.
FIGURE 1 » Representative structure of alpha-1,3-glucan.

This enzymatic polymerization process yields a polymer with high selectivity containing >99% alpha-1,3 linkages and with high compositional consistency (Figure 1). Using this technology, the alpha-1,3-polyglucose (glucan) structure can be controlled, with different levels of crystallinity (Figure 2), resulting in controlled spherical aggregates similar to fumed silica or submicron platelet-like particles (microcrystalline glucan, MCG).

Representative structures of glucan and aggregation into particles with different morphology and crystallinity levels.
FIGURE 2 » Representative structures of glucan and aggregation into particles with different morphology and crystallinity levels.

The resulting polysaccharides have repeat units that contain primary and secondary hydroxyl groups, which have been shown to be reactive with isocyanates, making them a potentially viable reactive additive in syntheses of polyurethanes, including water-based PUDs. In a model thermoplastic urethane system it has been shown that glucan impacts the polyurethane matrix morphology by forming a new covalent and hydrogen-bonded hard segment that strongly improves the solvent resistance of TPUs. Similarly, isocyanate-reactive glucan was shown to enhance the load-bearing properties of visco-elastic polyurethane foams.

Unlike water-soluble starch and water-insoluble cellulose, the glucan is also water-insoluble powder with sufficient affinity to water to produce stable water dispersions. As a result, the glucan morphologies are readily suited for incorporation into water-based PUDs. In water-based PUDs, the glucan can be utilized as an isocyanate reactive component in the synthesis of the polyurethane matrix. However, due to its water dispersability, glucan can also be added to a finished water-based PUD system, where these glucans are expected to impact the properties of the resulting films and coatings. Therefore, the aim of this study it to quantify the impact of enzymatically produced alpha-1,3 polyglucose of different morphologies on the performance of water-based PUDs, and to establish the impact of the glucan morphology and performance of the resulting polyurethane matrix.

 

Experimental

 

Materials

The discussed morphologies of glucan used in this study are prepared and supplied by IFF.

The glucan wet cake is the basic form of the alpha-1,3-polyglucose materials derived from the enzymatic polymerization of sugars, and typically contains about 35 wt.% solids, with the balance comprised of water. Prior to use for this study, glucan wet cake powder was dispersed in water, creating a 10 wt.% polysaccharide dispersion.

MCG is a highly crystalline form of alpha-1,3-polyglucose and was received as 8% dispersion in water.

1K water-based dispersions were supplied by Troy Polymers. The dispersions are based on high-renewable-content, sebacate-based polyester polyols.

 

Glucan/PUD Blends Preparation

Glucan was added to 1K-PUD at varying ratios. The mixture was first blended in a closed cup via multi-axial speed mixer for 1 minute, followed by wet milling for 1 minute via IKA mill.

The glucan/PUD mixtures were used to produce stand-alone films and coatings on aluminum. Using a Dr. Blade at 30 mils thickness, stand-alone films were prepared by coating the dispersion blend mixtures onto a polypropylene substrate. Similarly, glucan/PUD mixtures were coated onto aluminum substrates.

The films and coatings were allowed to dry for 24 hours at room temperature, followed by 24 hours at 50 °C. The films and coatings were conditioned for at least two additional days prior to testing.

 

Glucan/PUD Blends Testing

 

Glucan/PUD Films Testing

Tensile strength and elongation at break were determined using Instron equipped with heating chamber (5500R, Model 1122) following ASTM D2370. Stress-strain properties of PUD-based films were also measured upon hydrolytic aging in a moisture chamber at 95% relative humidity, 50 °C for 3 days.

Thermal properties of films were measured using differential scanning calorimetry (DSC) (Q10, TA Instruments). DSC analysis of TPU was carried out over the temperature range of -100 to 200 °C at the heating rate of 10 °C/min. In the first run, the TPU sample was heated from room temperature to 150 °C. The sample was then cooled down to -100 °C and heated to 200 °C (second run). The results from the second DSC run were reported.

FTIR spectra of TPUs were recorded on a Perkin Elmer Spectrum 100 equipped with Universal ATR Attachment, recording the spectra over a wavenumber range of 650 to 4,000 cm-1. The average value of 16 scans with 4 cm-1 resolution was collected for each sample.

 

Glucan/PUD Coatings on Aluminum Testing  

Gloss was determined at 60° angle using a gloss meter (ETB-0686 from M&A Instruments). Hardness was determined via pencil hardness method per ASTM D3363. Impact resistance was measured according to ASTM D2794. Adhesion was assessed via tape test per ASTM D3359. The hardness and adhesion of coatings cast on metal substrate was measured after hydrolytic aging in a moisture chamber for 3 days, 38 °C and 95% relative humidity ASTM D 2247.

 

Results

 

PUD with MCG Dispersion and Derived Films

MCG is the highly crystalline form of the polysaccharide materials and was received as 8% dispersion in water. MCG was added directly to PUDs, forming stable dispersions. Subsequently, PUD/MCG blends were cast on aluminum plates or cast onto polypropylene to form stand-alone films.

Interestingly, fully transparent and flexible films were obtained with up to 50% MCG content on dry film bases (Figures 3 and 6). Tensile properties of these films plotted as the concentration of MCG on dry film bases are shown in Figures 4 and 5. As expected, tensile modulus of the films increased with the addition of MCG. However, interestingly, tensile elasticity of the films essentially remained unaffected with the addition of up to 10% of MCG on dry film bases. Even with the addition of up to 40% MCG the films were quite elastic, with about 290% elongation at break.

PUD films with varying concentrations of MCG (from left to right: 0% MCG, 1% MCG, 3% MCG, 7% MCG and 10% MCG).
FIGURE 3 » PUD films with varying concentrations of MCG (from left to right: 0% MCG, 1% MCG, 3% MCG, 7% MCG and 10% MCG).

After hydrolytic age, modulus and elasticity of the referent film and films containing MCG decreased somewhat. However, elasticity of films improved, especially with the films containing higher levels of MCG. As a result, films containing 50% MCG became highly flexible, with elongation at break of about 290% (Figures 5 and 6).

Effect of hydrolytic aging (3 days at 50 °C and 95% RH) on tensile modulus at 100% elongation of PUD films containing MCG (micronized glucan).
FIGURE 4 » Effect of hydrolytic aging (3 days at 50 °C and 95% RH) on tensile modulus at 100% elongation of PUD films containing MCG (micronized glucan).
Effect of hydrolytic aging (3 days at 50 °C and 95% RH) on elongation of PUD films containing MCG (micronized glucan).
FIGURE 5 » Effect of hydrolytic aging (3 days at 50 °C and 95% RH) on elongation of PUD films containing MCG (micronized glucan).
Photo of free-standing film with 50% MCG in PUD on dry film bases after 3-day humid age at 50 ˚C.
FIGURE 6 » Photo of free-standing film with 50% MCG in PUD on dry film bases after 3-day humid age at 50 ˚C.

 

PUD with Wet Cake Dispersions and Derived Films

The alpha-1,3-polyglucose wet cake is the high surface area spherical morphology produced via the enzymatic polymerization of sugars. 10% glucan wet cake dispersion was added directly to PUDs, forming stable dispersions with a slow rate of settling (essentially stable). Subsequently, PUD films containing various levels of glucan wet cake were coated onto aluminum plates or cast onto polypropylene to form stand-alone films.

The addition of 10% glucan wet cake to PUDs resulted in an increase in viscosity (Figure 7). Due to this, the largest content evaluated was 15% glucan wet cake on dry film comparison base.

Effect of glucan wet cake concentration on viscosity of PUD blends.
FIGURE 7 » Effect of glucan wet cake concentration on viscosity of PUD blends.

As expected, the tensile modulus of the films increased with the addition of glucan wet cake. However, interestingly, tensile elasticity of the films was minimally affected with the addition of glucan wet cake, with films containing 15% of glucan wet cake having 600% elongation at break.

After hydrolytic age, modulus and elasticity of the referent film decreased somewhat. However, in general, both modulus and elasticity of films improved with increased content of glucan wet cake. Detailed analyses of tensile properties after hydrolytically aging of films shows that with increased content of glucan wet cake, tensile strength, modulus and elasticity increase, resulting in significant increase in film toughness (measured by area under stress-stain curves) (Figures 8 and 9, and Table 1).

 Effect of hydrolytic aging (3 days at 50 °C and 95% RH) on tensile modulus at 100% elongation of PUD films containing glucan wet cake.
FIGURE 8 » Effect of hydrolytic aging (3 days at 50 °C and 95% RH) on tensile modulus at 100% elongation of PUD films containing glucan wet cake.
Effect of hydrolytic aging (3 days at 50 °C and 95% RH) on tensile elasticity of PUD films containing glucan wet cake.
FIGURE 9 » Effect of hydrolytic aging (3 days at 50 °C and 95% RH) on tensile elasticity of PUD films containing glucan wet cake.
Hydrolytic aged properties of PUD films with varying amounts wet cake.
TABLE 1 » Hydrolytic aged properties of PUD films with varying amounts wet cake.

 

PUD with MCG Coatings

PUDs with various levels of MCG were coated onto aluminum and steel plates, and evaluated for key properties. The addition of MCG had no measurable impact on the impact resistance of the coatings. Also, the addition of MCG had no significant impact on the hardness of the coatings. Adhesion strength of PUDs on steel, as measured by tape test, was slightly improved with the addition of MCG. Adhesive strength to aluminum was slightly reduced with the addition of 20% MCG, however, cohesive mode of failure was maintained. Tables 2 and 3 show these results.

Properties of PUD coatings on steel substrate with MCG.
TABLE 2 » Properties of PUD coatings on steel substrate with MCG.
Adhesive properties on aluminum — PUDs with varying amounts of MCG.
TABLE 3 » Adhesive properties on aluminum — PUDs with varying amounts of MCG.

 

PUD with Wet Cake Coatings

PUDs with various levels of glucan wet cake were coated onto aluminum plates and evaluated for key properties. As shown in Table 4, the adhesive strength to aluminum as measured by load at failure was not affected. However, the mode of adhesive failure was improved. Whereas reference films experienced adhesive failure, films with glucan wet cake experienced cohesive failure.

The addition of glucan wet cake had no measurable impact on the impact resistance of the coatings. Also, the addition of glucan wet cake had no significant impact on the hardness of the coatings. Only at 15% glucan wet cake incorporation on dry film base was a slight reduction in hardness of coatings applied on aluminum observed. It should be noted that the hardness of coatings actually increased with the addition of glucan wet cake on the various substrates, such as for example wood.

Chemical resistance of the coatings was evaluated via rub-test with IPA and toluene. The addition of glucan wet cake was found to have essentially no negative impact on the chemical resistance to IPA and only slight decrease in resistance to toluene (Table 5).

Analysis of the coatings indicates that the addition of glucan wet cake decreases the gloss of the coatings (Figure 10). Therefore, it is possible that glucan wet cake can be utilized as a matting agent if that is desired in addition to the observed other property benefits. Having a matting agent that also enhances mechanical properties of films would be beneficial in a broad range of applications, including wood, textile and leather coatings.

Adhesive properties of PUDs with varying amounts of glucan wet cake.
TABLE 4 » Adhesive properties of PUDs with varying amounts of glucan wet cake.
Properties of PUD coatings with varying amounts of glucan wet cake on steel.
TABLE 5 » Properties of PUD coatings with varying amounts of glucan wet cake on steel.
Effect of glucan wet cake on gloss properties of films.
FIGURE 10 » Effect of glucan wet cake on gloss properties of films.

 

Wood Coating Evaluation

PUDs with various levels of glucan wet cake and MCG were coated onto oak and evaluated for key properties. The addition of glucan wet cake and MCG to the base PUD reduced the tackiness of the coating, providing a hand feel comparable to commercial wood coating. The addition of glucan wet cake reduced the gloss of coatings measured on wood, while the addition of MCG had no impact on gloss. Therefore, when matt finish is required, glucan wet cake can be used. When higher gloss finishes are required, MCG offers a better choice (Figure 11).

Photo of wood strip coated with referent PUDs: PUD+10% wet cake, PUD+12% wet cake, PUD+10% MCG, PUD+20% MCG, PUD+30% MCG, PUD+40% MCG, PUD+40% MCG (from left to right).
FIGURE 11 » Photo of wood strip coated with referent PUDs: PUD+10% wet cake, PUD+12% wet cake, PUD+10% MCG, PUD+20% MCG, PUD+30% MCG, PUD+40% MCG, PUD+40% MCG (from left to right).

Scratch resistance of the PUD coatings on wood was not affected with the addition of glucan wet cake and MCG. Coatings with up to 60% MCG and 30% glucan wet cake maintained scratch hardness of 7H-8H, which is significantly higher than 1H scratch resistance hardness measured for commercial water-based PUD wood coating (Tables 6a and 6b).

Additionally, rub test indicates that the addition of glucan wet cake and MCG improved the resistance of PUDs to IPA and water. It was found that the addition of either form of glucan resulted in reduced weight loss resulting from rub test to IPA. Coatings with up to 60% MCG and 30% glucan wet cake maintained lower weight loss during the rub test with IPA than commercial water-based PUD protective wood coating. Water drop test also indicates that wood coatings containing glucan wet cake and MCG offer potentially better protection than the reference commercial wood coating (Tables 6a and 6b).

Properties of PUD with MCG on oak samples.
TABLE 6a » Properties of PUD with MCG on oak samples.
Properties of PUD with glucan wet cake coatings on oak samples.
TABLE 6b » Properties of PUD with glucan wet cake coatings on oak samples.

 

Summary

Alpha-1,3-polyglucose glucan wet cake and MCG were evaluated as additives to 1K-PUDs. It was demonstrated that the addition of high levels of glucan wet cake and MCG to PUDs resulted in increased modulus of films while maintaining high levels of elasticity. Although hygroscopic, both glucan wet cake and MCG improved the hydrolytic resistance of PUD films, resulting in increase elasticity while maintaining higher tensile modulus and toughness compared to the reference PUD. As a result, after humid age films containing 50% MCG had almost 300% elongation at break.

It was demonstrated that the addition of high levels of glucan wet cake and MCG on PUDs had negligible impact on the properties of coatings on metal substrates. It was demonstrated that glucan wet cake and MCG had no significant impact on hardness, adhesion strength, impact resistance, or resistance to polar or non-polar solvents. However, PUDs with high levels of glucan wet cake or MCG showed promising performance on wood coatings, outperforming the commercial water-based 1K-PUDs in both the scratch resistance and water-resistance tests.

*This paper was presented at the 2021 Polyurethanes Technical Conference.

KEYWORDS: Polyurethane Resins PUDs

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Jorge Mok, Research Scientist, IFF, Wilmington DE
Christian Lenges, Venture Director, IFF, Wilmington DE
Natnael Behabtu, Global Biomaterials Application Leader, IFF, Wilmington DE
Ibrahim Sendijarevic, Business Development Director, Troy Polymers Inc., Troy, MI
Dr. Aisa Sendijarevic, Research Director; Troy Polymers Inc., Troy, MI

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • Double exposure of creative chemistry concept on laptop background, research and development concept

    Inside the AI Shift in Coatings

    Industry leaders share real-world examples of how AI is...
    Paint and Coating Equipment
    By: PCI Editorial Staff
  • Global Top 10 and PCI Logo

    2026 Global Top 10: Top Paint and Coatings Companies

    See how the world’s largest paint and coatings companies...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • The 2026 PCI 25

    2026 PCI 25: Top Paint and Coatings Companies

    See how North America's largest paint and coatings...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • Join Paint & Coatings Industry
  • Manage My Preferences
  • Customer Service

More Videos

Popular Stories

Mergers and aquisitions

BASF Ends Evonik Takeover Pursuit

Breaking News

H.B. Fuller to Close Seven Sites in Supply-Chain Overhaul

AkzoNobel Axalta

EU Clears $25B Akzo-Axalta Merger with One Big Condition

Events

December 2, 2026

Self-Activated Binder Technology: A New Path to Tin-Free Polyurethane Coatings

Through examples from protective and general industrial coating applications, attendees will learn how these innovative technologies can help maintain, and in some cases improve, coating performance while supporting safer, more sustainable formulations that align with evolving regulatory expectations

December 10, 2026

PC Academy: Waterborne Polymers and Film Formation

The trend towards waterborne polymers in the paint and coatings industry is clear; highlighting their environmentally friendly nature, regulatory considerations, growing market demand, and meeting sustainability goals.

View All Submit An Event

Products

Powder Coatings - Foundation for the Novice Formulator (ebook)

Powder Coatings - Foundation for the Novice Formulator (ebook)

See More Products
PCI news now promo ad

Related Articles

  • Natural Oil Metathesis Unlocks High-Performance Building Blocks for Waterborne Coating Additives and Polyurethane Dispersions

    Natural Oil Metathesis Unlocks High-Performance Building Blocks for Waterborne Coating Additives and Polyurethane Dispersions

    See More
  • taminco

    Waterborne Polyurethane Dispersions with New Sustainable Solvent

    See More
  • Stahl opens new facility.jpg

    Stahl Opens New Facility for Polyurethane Dispersions in Singapore

    See More

Related Directories

  • BASF Corp., Dispersions, Resins & Additives

    BASF offers a strong portfolio of industry-leading additives for the Coatings Industry to deliver eco-efficient solutions that meet performance requirements. The BASF Performance and Formulation additives portfolio encompasses a technology base of dispersing agents, wetting agents and surface modifiers, defoamers, rheology modifiers, film forming agents, antioxidants, light stabilizers and UV absorbers.
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Manufacturing Division
  • JOIN TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing