Painting & Coating Industry (PCI) logo Powder coating summit logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Painting & Coating Industry (PCI) logo Powder coating summit logo
  • NEWS
    • Latest News
    • Market Trends & Reports
    • Finishing News
    • Price Alerts
    • Subscribe to Newsletters
    • Global Top 10/ PCI 25
    • Weekly Featured Article
    • COATLE Word Game
  • PRODUCTS
    • Product News
    • Featured Products
    • Must See Products and Services
  • MATERIALS
    • Additives
    • Resins/Polymers
    • Pigments
    • Equipment
    • Distributors
  • TECHNOLOGIES
    • Adhesives
    • Architectural Coatings
    • Finishing Articles
    • Finishing Technologies
    • Finishing Equipment
    • Industrial Coatings
    • Nanotechnology
    • Powder Coatings
    • Solventborne
    • Special Purpose Coatings
    • Sustainability
    • UV Coatings
    • Waterborne
  • RESOURCES
    • Columns
      • Did you know?
      • Distribution Dive
      • Formulating With Mike
      • Innovation Insights
      • Powder Coating Perspectives
      • TiO2 Insider
    • Blogs
      • Editor's Viewpoint
      • Industry Insights
    • Coatings Supplier Handbook
    • Podcasts and Videos
      • COAT-IT! Podcast
      • Videos/PCI TV
    • PCI Store
    • Classifieds
    • eBooks
    • Sponsor Insights
    • White Papers
    • COATLE Word Game
  • EVENTS
    • Coatings Trends & Technologies Summit
    • Paint and Coatings Academy
    • Webinars
    • Calendar of Events
    • Lifetime Achievement Award
  • DIRECTORIES
    • Buyer's Guide
    • Equipment Directory
    • Materials Directory
  • EMAGAZINE
    • Current Issue
    • eMagazine Archive
    • China Issue Archive
    • Editorial Advisory Board
  • CONTACT
    • Contact Us
    • Advertise
    • Subscribe to eMagazine
    • Subscribe to Newsletters
  • SIGN UP!
Paint and Coating Resins & PolymersIndustrial CoatingsSpecial Purpose CoatingsWaterborne Coatings

Waterborne Epoxy Zinc-Rich Primers: There Are Viable Options

By Françoise Heine, Pascale Bouuaert, Nathalie Wauters, Jim Elmore, Bedri Erdem, Derek Crawford
pci0912-Mo-F1-615.jpg
Credit: Hexion Inc.
pci0912-Mo-F2-615.jpg
Credit: Hexion Inc.
pci0912-Mo-F3-615.jpg
Credit: Hexion Inc.
pci0912-Mo-F4-615.jpg
Credit: Hexion Inc.
pci0912-Mo-F5-615.jpg
Credit: Hexion Inc.
pci0912-Mo-T1-615.jpg
Credit: Hexion Inc.
pci0912-Mo-F1-615.jpg
pci0912-Mo-F2-615.jpg
pci0912-Mo-F3-615.jpg
pci0912-Mo-F4-615.jpg
pci0912-Mo-F5-615.jpg
pci0912-Mo-T1-615.jpg
September 4, 2012
With stringent environmental and health regulations, waterborne coatings are increasingly replacing solventborne paints. Significant advances have been made: new waterborne epoxy resin and amine curing agent technologies provide excellent corrosion resistance when appropriate two-component (2K) formulations are used.

In the specific case of epoxy primers enriched with zinc for extra corrosion resistance, the challenge of incorporating a very high weight (often 80-85%) of zinc powder into an epoxy/curing agent binder system is compounded by zinc’s reactivity with protic components such as water, acidic solvents and dispersing aids.

 We have developed and tested several 2K waterborne epoxy/amine systems designed to improve pigment loading and to protect zinc from protic media that cause hazardous hydrogen generation. These new systems have been tested against classical solventborne and waterborne epoxy systems. The preferred system provides a storage-stable, 2K zinc-rich coating with a long pot life. It yields a flexible coating that provides steel with excellent corrosion protection at much lower VOC levels (~200 g/L) than solventborne systems. This article provides an overview of this novel 2K waterborne epoxy binder system that allows formulation with high levels of zinc.

Waterborne Epoxy Technologies Overview1,2

In early waterborne technologies, the epoxy resin was simply dispersed and stabilized in water (Figure 1). In more recent waterborne epoxy technologies, the dispersant and stabilizers are chemically reacted onto the backbone of the epoxy polymers rather than just blended with the resin. In both cases, the amine curing agent is usually a water-dilutable polymer.

NewGen™ epoxy-amine waterborne technology (Figure 2) was designed to replace solventborne epoxy-polyamide coating technology. The epoxy (EPI-REZ™ Resin 6520-WH-53) is self-emulsified, contains no free surfactants, and is crosslinked with a unique, zero-VOC amine curing agent dispersion (EPIKURE™ Curing Agent 6870-W-53). This NewGen system allows formulation of fast-drying, highly corrosion resistant, <100 g/L VOC, ambient-cure primers and direct-to-metal protective coatings.

Performance

The corrosion resistance delivered by this system is illustrated in Figure 3. The coating was sprayed onto sand-blasted steel panels, cured for one week at room temperature and then exposed to salt spray and continuous condensation for 1000 h. After 300 h of salt spray and continuous condensation exposure, the NewGen formulation displayed excellent corrosion resistance as well as superior adhesion to cold rolled steel.

But what if we wanted even better corrosion resistance while still conforming to the new regulations? Adding zinc to solventborne primers enhances their corrosion resistance. Is it possible to make a waterborne 2K, low-VOC, corrosion-resistant epoxy primer system that outperforms commercial solventborne epoxy zinc-rich primers?

What Are the Challenges?

In aqueous formulations, zinc reacts with water, forming zinc hydroxide and releasing hydrogen (eq 1).

Zn + 2H2O àZn(OH)2 +H2 á↑                             [1]

Because of this, the main challenge in creating a zinc-rich waterborne primer is to prevent the zinc from reacting with water during storage and application. Adding untreated zinc dust directly into aqueous components must be avoided to prevent the hazards associated with hydrogen generation.

Evolving Methodologies

Waterborne 3K systems are available, with the zinc being added as a third component to the aqueous binder just before paint application. This approach is complicated by the need for proper mixing of multiple components, as well as the potential health and safety issues regarding inhalation when incorporating powdered zinc. It is typically limited to the use of 2K coatings with 1 h application lives.

For easier application of waterborne zinc-rich epoxy coatings it is necessary to protect the zinc from the water, without deactivating it. The zinc metal must still be available as a sacrificial oxidant to protect the iron-containing substrates being coated.

One approach to this problem is described by Momentive Performance Materials.3,4 A zinc-rich paste was made by dispersing the zinc dust into a silane hydrolyzate, which protects the zinc and prevents it from reacting with water. Then the epoxy dispersion was added to this slurry. Another variation is to disperse the zinc dust into a pre-mix of the silane hydrolyzate and the epoxy resin dispersion.

The stability of these zinc pastes was tested by measuring for hydrogen outgassing at 40 °C. The 3K formulation failed after a few hours. The 2K silane hydrolyzates were significantly more stable at ambient temperature for up to 6 months. However, they exhibited some hydrogen outgassing when stored at 40 °C. Thus, more work was needed to develop a 2K zinc-rich primer that was stable even at elevated temperatures.

What if the zinc were added to the amine curing agent instead of the epoxy resin component? “Hybrid” waterborne epoxy systems have been developed in which zinc is dispersed in a high-solids, non-aqueous amine curing agent. This zinc-rich curing agent is then combined with a waterborne epoxy dispersion to form a 2K coating. Unfortunately, after the two components are mixed, hydrogen outgassing often begins quite strongly and the working pot life is not very long. Clearly, a new modified curing agent needed to be developed.

Preferred Approach

A new water-free amine − EPIKURE Curing Agent 8538-Y-68 − has been designed for use in waterborne zinc-rich primers. This amine curing agent works by quickly saturating the zinc surface with reactive hydrophobic polymers that encapsulate and protect the zinc from water. It performs well even in primers loaded with 80% zinc by weight. Once the amine components are reacted with the epoxy, the zinc surface again becomes available as a sacrificial electrolytic surface to form oxides that act as a corrosion barrier for iron-containing substrates. By using EPIKURE Curing Agent 8538-Y-68 in a highly filled zinc paste, with the appropriate waterborne epoxy dispersion, more than 4 h of working pot life is achieved with no outgassing.

 The advantages of this new amine curative for use in epoxy zinc-rich primers are:

•   Easier dispersion of the zinc powder;

•   High-solids, acid-free and non-aqueous amine to minimize outgassing with zinc;

•   Shelf stable: very limited to no detectable outgassing during zinc paste storage;

•   Pot life: significantly longer pot life than other waterborne zinc alternatives;

•   Suitable for use in non-zinc coating systems;

•   Excellent intercoat adhesion with other waterborne mid- and topcoats;

•   Excellent corrosion protection.

For best performance, this new amine curative should be combined with a stable dispersion of solid epoxy resin in water. The choice of epoxy dispersion resin is critical for obtaining long pot life, good paint coalescence and adequate crosslinking. Based on a survey of commercial dispersions, EPI-REZ Resin 6520-WH-53 was determined to be the best option. Care should also be taken to select non-acidic additives, particularly for the EPIKURE Curing Agent 8538-Y-68 zinc paste. An example of a formulation with superior performance is given in Table 1.

This formulation can be made to dry very quickly by selecting appropriate alcohol and glycol ether solvents. Typically this formulation has a pot life of at least 4 h. Recoat times can be minimized to only a few minutes if adequate air flow is available to accommodate water evaporation. There is no significant hydrogen outgassing during pot life, thus allowing a continuous coating barrier to be applied to protect the metal substrate.

As seen in Figure 4, salt spray-exposed steel panels coated with the formulation in Table 1 protect metal significantly better than the solventborne zinc-rich primer seen in Figure 5. This shows that the zinc is available for corrosion protection, even if significant outgassing is not observed during the pot life.               

Conclusions

Zinc-rich 2K waterborne epoxy primers are now possible using new amine technology (EPIKURE Curing Agent 8538-Y-68). At the same zinc loading, the corrosion performance using this curing agent with solid epoxy dispersions is comparable to, or better than, that achieved with traditional solventborne epoxy/polyamidoamine binders.

The zinc-rich paste based on this new curing agent shows no significant outgassing when the curing agent and epoxy components are mixed. Resulting pot life with the recommended solid epoxy dispersion is at least 4 h.

The superior metal protection of NewGen-type, waterborne, 2K epoxy binder systems has been extended via a new curing agent technology that is suitable for highly filled zinc-rich primer formulations. This route allows significant VOC reduction in the important application area of organic zinc-rich primers.

 

References

1  Heine, F., et al. Waterborne Epoxy Technologies, EuRAILmag, Oct., 2007.

2Elmore, J., et al. WB Epoxy Protective Coatings for Metal, JCT, Vol 74, No 931, Aug., 2002.

3Heine, F., et al. Waterborne epoxy coatings in the marine industry: an option?, Nürnberg Coating Show 2009.

    4  Lejeune, A., et al. New class of epoxy functional silanes for uses in coatings, adhesives and sealants: epoxy silane oligomers, 21st National OCCA                            Symposium in conjunction with SAPMA, Oct., 2006.n

KEYWORDS: Epoxy Resins Metal Coatings

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Françoise Heine, Hexion Inc., Stafford, TX
Hexion Specialty Chemicals, Stafford, TX

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • pci1022-Kinaltek-Lead-1170.jpg

    A Novel Pigment Production Technology

    Following an extensive R&D program that demonstrated...
    Paint and Coating Pigments
    By: Jawad Haidar and Nitin Soni
  • pci global top 10

    2025 Global Top 10: Top Paint and Coatings Companies

    The following is PCI’s annual ranking of the top 10...
    Global Top 10 and PCI 25
    By: Courtney Bassett
  • 2025 pci 25

    2025 PCI 25: Top Paint and Coatings Companies

    PCI's annual ranking of the top 25 North American paint...
    Global Top 10 and PCI 25
    By: Courtney Bassett
You must login or register in order to post a comment.

Report Abusive Comment

Manage My Account
  • eMagazine
  • Newsletters
  • Online Registration
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the PCI audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of PCI or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • wooden kitchen set and shelving
    Sponsored bySirca North America

    Leveraging Coatings to Meet ESG Goals in Manufacturing

  • man woodworking in workshop
    Sponsored byGemini Industries, Inc.

    Waterborne Coatings Aren't the Future -- They're the New Performance Benchmark

  • colorful building exterior
    Sponsored byDow

    Insights into Exterior Architectural Coating Degradation: Bridging Accelerated and Natural Weathering

Popular Stories

Supply chain question and cargo piles up and piling shipping containers question concept

Energy Disruptions Begin to Hit Coatings Supply Chain

basf

BASF Coatings Names Incoming CEO Ahead of Separation

White bay windows and French doors

Enhancing Block Resistance in Low-VOC Acrylic Paints Using Silane-Modified Colloidal Silica

POB-Point-and-Shoot

PCI Buyers Guide

Submit a Request for Proposal (RFP) to suppliers of your choice with details on what you need with a click of a button

Start your RFP

Browse our Buyers Guide for manufacturers and distributors of all types of coatings products and much more!

Find Suppliers

Events

September 4, 2025

N-Butylpyrrolidone (NBP) as a Green Solvent to Replace N-Methylpyrrolidone (NMP) in Industrial Coating Applications

ON DEMAND: EPA published a regulation proposal around N-methylpyrrolidone (NMP) in June 2024 to ban or limit NMP in many applications, such as paints and coatings and their removers. N-butylpyrrolidone (NBP) is a powerful and versatile solvent for a variety of industries looking for alternatives to substance of very high concern (SVHC)-listed solvents.

April 28, 2026

Next Gen Dispersion Technology in Paint Production: Driving Higher Quality at Lower Costs

Join this webinar to see how manufacturers reduce costs, energy use, raw materials, labor, and floor space while improving quality.

View All Submit An Event

Poll

Longest-running laboratory experiment

What is the longest-running laboratory experiment?
View Results Poll Archive

Products

Automotive Paints and Coatings, 2nd Edition

Now in its second edition and still the only book of its kind, this is an authoritative treatment of all stages of the coating process.

See More Products
Register for webinar: Next-Gen Dispersion Technology in Paint Production

Related Articles

  • The arch of the Humber River Walk Bridge in Toronto, Ontario

    Zinc-Rich Primers

    See More
  • Zinc-Rich Primers With Micaceous Iron Oxide

    See More
  • protective coatings

    Sherwin-Williams Launches Organic Zinc-Rich Epoxy Coating

    See More
×

Keep the info flowing with our eNewsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Store
    • Want More
    • Manufacturing Division
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing